ACI Field Testing I Practice Test

ACI Concrete Field Testing Technician-Grade I

ACI Field Testing I overview

  • 200 practice questions
  • 32 flashcards
  • 8 study guide topics
  • 39 key terms

What you'll study

  • Sampling Freshly Mixed Concrete13%
  • Temperature of Freshly Mixed Concrete13%
  • Slump of Hydraulic Cement Concrete13%
  • Density (Unit Weight), Yield, and Air Content (Gravimetric) of Concrete13%
  • Air Content of Freshly Mixed Concrete by the Pressure Method12%
  • Air Content of Freshly Mixed Concrete by the Volumetric Method12%
  • Making and Curing Concrete Test Specimens in the Field12%
  • Capping and Compressive Strength Testing of Cylindrical Specimens12%

The ACI Concrete Field Testing Technician-Grade I is an entry-level credential for people who sample and test freshly mixed concrete on construction sites. ACI lists it among its Field Concrete Testing programs, within a certification portfolio of over 30 programs designed to form a minimum qualification for personnel employed within the concrete construction industry. Examinations, and optional training courses, are conducted through an international network of over 135 sponsoring groups, so scheduling and logistics run through a local sponsor rather than a single central venue. Candidates face two components: a multiple-choice paper and a hands-on performance test in which they carry out standard field procedures and report results. The published domain outline splits into eight areas - sampling, temperature, slump, density/yield/gravimetric air content, pressure-meter air content, volumetric air content, making and curing specimens, and capping and compressive testing - each weighted between 12 and 13 percent, so there is no safe topic to skip. Preparation usually means practising the physical procedures with the actual apparatus until they become automatic, then drilling the written material behind each one. Because pass marks, fees, and retake rules are not published on the ACI program pages, confirm those details with your sponsoring group before booking.

Common mistakes

Collecting the sample only from the first portion of the discharge or scooping from the top of the wheelbarrow, rather than combining increments across the middle of the discharge.

The first and last concrete out of a mixer or truck is richer or leaner in mortar and aggregate; a single-point sample cannot represent the batch, and top scooping biases the sample toward paste, shifting slump, air, and strength results.

What to do instead

Take at least three increments at approximately equal intervals over the middle 1/2 to 2/3 of the discharge, catch them in a clean, dampened wheelbarrow, and combine; do not sample from the very beginning or end unless the specification requires it.

Beginning slump, air, or density tests on a sample that has not been remixed, or allowing the sample to sit beyond the allowed time before testing.

Concrete segregates and loses workability after sampling; testing an undisturbed sample gives a non-representative slump and air content, and delayed testing lets absorption and evaporation change results.

What to do instead

Remix the sample with a shovel for about 30 s before each test, start tests promptly (within 15 min of sampling per C172), complete them within the allowed interval, and discard and resample if the sample has stiffened or segregated.

Inserting the thermometer only about 25 mm (1 in.) into the concrete and reading it immediately after insertion.

A shallow or short immersion measures the surface temperature, which is affected by air and container, and the thermometer needs time to equilibrate; immediate readings are biased high or low.

What to do instead

Insert the thermometer at least 75 mm (3 in.) into the concrete, close the concrete around it, leave it for at least 2 min and no more than 5 min, and read while the stem is still immersed; measure within 15 min of sampling.

Rodding the slump cone with uneven strokes or through the full depth of each layer, and lifting the cone with a twist or in less than 5 s.

Uneven or excessive rodding overconsolidates some zones and leaves others honeycombed; through-rodding the upper layers over-compacts lower concrete; twisting or fast lifting drags the concrete and changes the slump.

What to do instead

Fill in three equal layers; rod each layer 25 strokes uniformly, with the bottom layer rodded through its depth and upper layers just into the previous layer; lift the cone vertically in 5 ± 2 s without lateral or twisting motion.

Using a unit-weight measure whose volume is assumed rather than calibrated, and filling it without the specified three layers and 25 strokes per layer.

A dented or uncalibrated measure introduces a fixed volume error into density and yield; poor consolidation leaves voids that lower unit weight and falsely raise yield.

What to do instead

Calibrate the measure by filling with water at a known temperature and calculating volume from the mass of water; fill in three equal layers, rod 25 strokes per layer for a 0.5 ft³ measure, tap the sides, strike off, and determine mass to the required precision.

Calculating yield from design batch weights or from an assumed air content instead of the actual batch weights and measured air content.

Yield is the actual volume produced per batch; using design weights hides over- or under-batching, and ignoring measured air changes the calculated density and volume.

What to do instead

Use the actual batch weights from the batch ticket, compute total mass, divide by the measured fresh density to get yield, and compare with the design volume; use the air content measured on the same sample.

Reading the pressure-meter gauge directly as total air content without applying an aggregate correction factor, or using a correction factor from a different aggregate source.

The pressure method measures air in the concrete plus air trapped in pores of the aggregate; without the source-specific correction, the gauge overstates the air content.

What to do instead

Determine the aggregate correction factor for the actual aggregate combination per C231, subtract it from the gauge reading, and re-determine it when aggregate sources or proportions change.

In the volumetric air test, reading the liquid level as soon as the meter is inverted a few times, before bubbles have stopped rising, or adding an arbitrary amount of alcohol.

Entrained air is released slowly; an early reading includes bubbles still in the liquid and underreads true air, while incorrect alcohol volume changes the liquid level and meniscus.

What to do instead

Add the specified amount of isopropyl alcohol, cap, invert and roll the meter for the required time, then let it stand until bubbles stop, tap the gauge, and read the bottom of the meniscus at eye level.

Leaving field cylinders exposed to sun, wind, or freezing temperatures during initial curing, or rodding them with the wrong layer and stroke pattern.

Rapid moisture loss or temperature extremes during the first 24 h cause surface cracking, incomplete hydration, and low strength; improper rodding creates voids or segregation.

What to do instead

Rod 6×12 in. cylinders in two layers with 25 strokes per layer (4×8 in. also two layers, 25 strokes), strike off, cover to prevent evaporation, cure initially at 60–80°F, and protect from freezing and vibration until demolding.

Testing a cylinder with a cap that is not perpendicular to the axis or is thicker than allowed, and applying load at a rate outside the specified range.

A tilted or thick cap introduces eccentric loading or a soft layer, causing premature failure; too-fast loading raises apparent strength and too-slow loading lowers it.

What to do instead

Cap with a flat plate and guide so the cap is perpendicular within tolerance and no thicker than 3 mm (1/8 in.) for sulfur mortar, then test at 0.25 ± 0.05 MPa/s (35 ± 7 psi/s) and center the specimen on the platen.

Exam requirements can change. Confirm current details with the exam provider.

ACI Field Testing I practice

200 questions. Each one lists the choices, the correct answer, and an explanation. With JavaScript, this list opens one question at a time. The checker at the top of this page saves progress in this browser when it is available.

  1. Question 1Sampling Freshly Mixed Concrete

    What is the minimum volume of a fresh concrete sample required for strength test specimens under ASTM C172?

    1. 1.00 ft³ (0.028 m³) Correct answer.
    2. 2.00 ft³ (0.057 m³)
    3. 0.50 ft³ (0.014 m³)
    4. 0.25 ft³ (0.007 m³)

    Explanation

    ASTM C172 requires a sample of at least 1 ft³ (0.03 m³) when strength specimens are to be made, so enough concrete is available for all tests. Smaller samples may not provide sufficient material for the required specimens.

  2. Question 2Sampling Freshly Mixed Concrete

    When sampling from a truck mixer, at what point in the discharge should the sample be obtained?

    1. From the top of the drum before discharge
    2. At the very end of the discharge
    3. From the first concrete out of the drum
    4. After 10% to 15% is discharged Correct answer.

    Explanation

    C172 specifies sampling after about 10% to 15% of the batch has been discharged so the sample is representative. The first and last portions may be segregated or contain excess water.

  3. Question 3Sampling Freshly Mixed Concrete

    For a stationary mixer, when should the sample be taken?

    1. From the first 5% of the discharge
    2. Before any concrete is discharged
    3. After about 10% is discharged Correct answer.
    4. After the entire batch has been discharged

    Explanation

    The sample should be obtained after approximately 10% of the batch has been discharged, from the middle portion of the discharge stream. This avoids the non-representative first and last portions.

  4. Question 4Sampling Freshly Mixed Concrete

    What tool should be used to remix a composite concrete sample before testing?

    1. A steel trowel
    2. A hand scoop
    3. A shovel Correct answer.
    4. A vibrating table

    Explanation

    C172 requires the composite sample to be remixed with a shovel before tests are performed to ensure uniformity. Trowels and scoops are too small for proper remixing of the full sample.

  5. Question 5Sampling Freshly Mixed Concrete

    What is the maximum time allowed between obtaining a sample and starting the tests?

    1. 30 minutes
    2. 15 minutes Correct answer.
    3. 5 minutes
    4. 10 minutes

    Explanation

    Tests should begin within 15 minutes after the sample is obtained to minimize changes in workability and air content. The sample must be protected during this interval.

  6. Question 6Sampling Freshly Mixed Concrete

    Adding water to a fresh concrete sample to adjust slump is:

    1. Permitted if done within 5 minutes
    2. Permitted if the sample is remixed for 2 minutes
    3. Not permitted at any time Correct answer.
    4. Permitted if cement is also added

    Explanation

    C172 prohibits adding water to the sample because it changes the water-cement ratio and makes the sample unrepresentative. The sample must be tested as obtained.

  7. Question 7Sampling Freshly Mixed Concrete

    How should a sample be obtained from a paving mixer?

    1. From the first material discharged from the mixer
    2. Three locations across the width, away from edges Correct answer.
    3. From the edges of the mat where segregation occurs
    4. From one location at the center of the mat

    Explanation

    C172 requires sampling from at least three locations across the width of the paving machine, avoiding the edges where segregation may occur. This produces a representative composite sample.

  8. Question 8Sampling Freshly Mixed Concrete

    When concrete is delivered by pump, where should the sample be taken?

    1. From the pump hopper
    2. From the top of the pump line
    3. From the first concrete out of the hose
    4. At the discharge end of the hose Correct answer.

    Explanation

    The sample should be obtained at the discharge end of the hose so it reflects the concrete as placed. The hopper and the first portion out of the hose may not be representative.

  9. Question 9Sampling Freshly Mixed Concrete

    A container used to hold a fresh concrete sample should be:

    1. Clean, damp, non-absorbent Correct answer.
    2. Coated with a release agent
    3. Made of untreated wood
    4. Dry and highly absorbent

    Explanation

    The container must be clean, damp, and non-absorbent to prevent loss of water or contamination. This helps preserve the sample's original characteristics.

  10. Question 10Sampling Freshly Mixed Concrete

    Why is the first portion of discharge avoided when sampling concrete?

    1. It is always colder than the rest of the batch
    2. It is needed only for slump testing
    3. It may be segregated or carry excess water Correct answer.
    4. It contains more cement than the rest

    Explanation

    The first concrete out of a mixer or truck may be segregated or carry excess water, so it is not representative of the batch. Sampling after 10% to 15% has been discharged avoids this problem.

  11. Question 11Sampling Freshly Mixed Concrete

    A composite concrete sample is best described as:

    1. A sample taken after all tests are complete
    2. A sample taken from a single point in the discharge
    3. A sample taken only from the top of the drum
    4. Portions taken from different locations and combined Correct answer.

    Explanation

    A composite sample combines portions from several locations or times in the discharge to represent the whole batch. The portions are then remixed before testing.

  12. Question 12Sampling Freshly Mixed Concrete

    When sampling from a conveyor belt, how should the sample be obtained?

    1. Take material only from the belt edges
    2. Full cross-section at three or more locations Correct answer.
    3. Take one large sample from the end of the belt
    4. Take a small scoop from the center of the belt

    Explanation

    C172 requires taking the full cross-section of the belt at three or more locations so coarse and fine particles are proportionally represented. Partial samples may miss segregated material.

  13. Question 13Sampling Freshly Mixed Concrete

    A fresh concrete sample should be protected from:

    1. Mixing with a shovel
    2. Evaporation and rapid drying Correct answer.
    3. Being placed in a damp container
    4. Testing within 15 minutes

    Explanation

    The sample must be protected from evaporation, wind, and direct sunlight because water loss changes slump and air content. Covering the sample is a common protective measure.

  14. Question 14Sampling Freshly Mixed Concrete

    Which source is acceptable for obtaining a fresh concrete sample?

    1. The top of a settled wheelbarrow
    2. The mixer or truck discharge stream Correct answer.
    3. A concrete stockpile left on the ground
    4. A pile of hardened concrete

    Explanation

    Samples must be taken from the discharge stream at the point of placement, not from stockpiles or settled containers. Stockpiles may be segregated or contaminated.

  15. Question 15Sampling Freshly Mixed Concrete

    The sample should be obtained at the:

    1. Point of discharge Correct answer.
    2. Bottom of the hauling unit
    3. Top of the mixer drum
    4. Point of mixing water addition

    Explanation

    C172 requires sampling at the point of discharge so the concrete tested matches the concrete delivered. Sampling elsewhere may not represent the batch.

  16. Question 16Sampling Freshly Mixed Concrete

    A properly obtained fresh concrete sample should represent:

    1. The top layer of the batch
    2. Only the first batch of the day
    3. The entire batch from which it is taken Correct answer.
    4. Only the concrete used for strength tests

    Explanation

    The purpose of sampling is to obtain a representative portion of the entire batch. All portions of the batch should have an equal chance of being included.

  17. Question 17Sampling Freshly Mixed Concrete

    When sampling from a stationary mixer, the container should be passed through the discharge stream at least how many times?

    1. Four times
    2. Two times
    3. One time
    4. Three times Correct answer.

    Explanation

    C172 requires passing the container through the discharge stream at least three times to build a representative composite sample. This helps include material from different parts of the stream.

  18. Question 18Sampling Freshly Mixed Concrete

    For a given set of tests, the sample should be taken from:

    1. The first batch of the day
    2. Several different batches combined
    3. A single batch Correct answer.
    4. The last batch of the day

    Explanation

    Each set of tests should represent one batch, so the sample should come from a single batch. Combining batches makes the results difficult to interpret.

  19. Question 19Sampling Freshly Mixed Concrete

    After obtaining a sample, it should be transported to the test area:

    1. Only after it has set slightly in the container
    2. In an open, sunny location near the site
    3. Promptly and protected from evaporation Correct answer.
    4. After adding a small amount of water to it

    Explanation

    The sample should be moved promptly and protected from evaporation to preserve its properties. Delays and water loss can change test results.

  20. Question 20Sampling Freshly Mixed Concrete

    When sampling from a chute, from which part of the discharge should the sample be taken?

    1. The last concrete out of the chute
    2. The first concrete out of the chute
    3. Concrete clinging to the chute sides
    4. Middle of the discharge stream Correct answer.

    Explanation

    The middle portion of the discharge is most representative because the first and last portions may segregate. The container should be passed through the stream several times.

  21. Question 21Sampling Freshly Mixed Concrete

    Why is sampling from a pump hopper not acceptable?

    1. The hopper concrete has already hardened
    2. The hopper is always dry inside
    3. The hopper is too small to hold a sample
    4. Hopper concrete may not be representative Correct answer.

    Explanation

    Concrete in the pump hopper may have segregated or changed due to pumping, so it may not represent the concrete delivered at the hose. The sample must be taken at the discharge end.

  22. Question 22Sampling Freshly Mixed Concrete

    Why should the edges of a paving mixer be avoided when sampling?

    1. Edges may be segregated and not representative Correct answer.
    2. The edges contain too much cement paste
    3. The edges are always too wet compared with the center
    4. The edges are too cold for sampling

    Explanation

    Edges of a paving mat can segregate, with coarse aggregate or fines concentrating there. Sampling across the width but away from edges gives a more representative composite.

  23. Question 23Sampling Freshly Mixed Concrete

    When concrete is delivered in a non-agitating truck, where should the sample be obtained?

    1. From the discharge stream Correct answer.
    2. From the top of the load
    3. From the first material dumped
    4. From the bottom of the truck bed

    Explanation

    Non-agitating trucks can segregate, so the sample must be taken from the discharge stream as the concrete is placed. Sampling from the top, bottom, or first material may not represent the load.

  24. Question 24Sampling Freshly Mixed Concrete

    Which portion of a mixer discharge should be avoided when sampling?

    1. The portion after 15% has been discharged
    2. The middle 50% of the batch
    3. The portion between 20% and 80% of discharge
    4. The first and last portions Correct answer.

    Explanation

    The first and last portions of a discharge can be segregated or contain excess water, so they are avoided. Sampling from the middle portion gives a more representative sample.

  25. Question 25Sampling Freshly Mixed Concrete

    If a sample must wait before testing, how should it be stored?

    1. In a dry, absorbent container
    2. With added water to keep it workable
    3. Covered and protected from drying Correct answer.
    4. In an open container in the sun

    Explanation

    The sample should be covered and protected from evaporation, wind, and sunlight during any wait. Adding water or using absorbent containers changes the sample.

  26. Question 26Sampling Freshly Mixed Concrete

    What is the minimum volume of a fresh concrete sample that should be obtained for routine field tests?

    1. About 1 ft³ (28 L) Correct answer.
    2. About 0.25 ft³ (7 L)
    3. About 2 ft³ (57 L)
    4. About 0.5 ft³ (14 L)

    Explanation

    Standard sampling practice requires a fresh concrete sample of at least 1 ft³ (28 L) for routine field tests. The sample must be large enough to complete all required tests and still have material left over, so the tests are not compromised by a shortage. A larger sample is needed when the nominal maximum aggregate size is large or when extra tests are specified.

  27. Question 27Temperature of Freshly Mixed Concrete

    According to the standard test method for temperature of freshly mixed concrete, a field thermometer must be accurate to within:

    1. ±0.5 °C (±1 °F) Correct answer.
    2. ±5 °C (±10 °F)
    3. ±2 °C (±4 °F)
    4. ±1 °C (±2 °F)

    Explanation

    The test method requires the thermometer to measure the temperature of fresh concrete to an accuracy of ±0.5 °C (±1 °F) across its working range. This tight tolerance is needed because the result is compared directly with specification limits such as 95 °F, where a coarse instrument could hide an excursion.

  28. Question 28Temperature of Freshly Mixed Concrete

    What is the minimum depth to which the sensing portion of the thermometer must be immersed in the concrete?

    1. 75 mm (3 in.) Correct answer.
    2. 25 mm (1 in.)
    3. 250 mm (10 in.)
    4. 150 mm (6 in.)

    Explanation

    The sensing portion must be submerged at least 75 mm (3 in.) below the concrete surface so that the reading reflects the concrete rather than the surrounding air or the container. Shallow immersion biases the result toward ambient conditions.

  29. Question 29Temperature of Freshly Mixed Concrete

    How long must the thermometer remain in the concrete before the temperature is read?

    1. 30 s
    2. 10 min
    3. 15 s
    4. 2 min Correct answer.

    Explanation

    The thermometer stays in the concrete at least 2 minutes, or until the reading becomes stable, so the sensing element reaches thermal equilibrium with the concrete. Reading earlier can capture a value that still reflects the air or the container.

  30. Question 30Temperature of Freshly Mixed Concrete

    To what precision is the concrete temperature read and recorded?

    1. 0.5 °C (1 °F) Correct answer.
    2. 2 °C (5 °F)
    3. 0.1 °C (0.2 °F)
    4. 1 °C (2 °F)

    Explanation

    The temperature is read and recorded to the nearest 0.5 °C (1 °F), which matches the accuracy the method requires of the instrument. Reporting a coarser value would lose meaningful information near a specification limit.

  31. Question 31Temperature of Freshly Mixed Concrete

    Which standard is the test method for temperature of freshly mixed hydraulic-cement concrete?

    1. ASTM C1064 Correct answer.
    2. ASTM C172
    3. ASTM C231
    4. ASTM C143

    Explanation

    ASTM C1064 is the standard test method for temperature of freshly mixed hydraulic-cement concrete. It covers the thermometer requirements, the measurement procedure, and the reporting of results.

  32. Question 32Temperature of Freshly Mixed Concrete

    Where should the sensing portion of the thermometer be positioned in a sample of fresh concrete?

    1. On the bottom of the container, where the concrete is coolest
    2. Just under the surface, no deeper than 25 mm
    3. In the interior, at least 75 mm from the container wall Correct answer.
    4. At the surface, where the reading responds fastest to air temperature

    Explanation

    The sensor belongs in the interior of the sample, at least 75 mm (3 in.) from the container wall, so neither the container nor the air controls the reading. Concrete is a poor conductor, so edge and surface locations can be noticeably off.

  33. Question 33Temperature of Freshly Mixed Concrete

    The thermometer used for this test must have a range that includes at least:

    1. −18 to 0 °C (0 to 32 °F)
    2. 0 to 25 °C (32 to 77 °F)
    3. 0 to 100 °C (32 to 212 °F)
    4. 0 to 50 °C (30 to 120 °F) Correct answer.

    Explanation

    The instrument must span at least 0 to 50 °C (30 to 120 °F) so it can cover both cold-weather and hot-weather concrete temperatures. A narrower span would not read hot-weather concrete.

  34. Question 34Temperature of Freshly Mixed Concrete

    Unless the project specifications state otherwise, the general maximum temperature of concrete at the time of placement is:

    1. 50 °C (120 °F)
    2. 35 °C (95 °F) Correct answer.
    3. 25 °C (77 °F)
    4. 40 °C (104 °F)

    Explanation

    The general upper limit for concrete at the time of placement is 35 °C (95 °F). Above that, workability, air content, and cracking tendency become harder to control.

  35. Question 35Temperature of Freshly Mixed Concrete

    A thermometer is checked in a properly prepared ice-water bath and reads 1.0 °C (34 °F). What is the correct action?

    1. Deduct 1.0 °C from each future reading and continue testing
    2. Use it, because an ice bath is not a valid field check
    3. Remove it from service until it is recalibrated or replaced Correct answer.
    4. Use it, since errors under 2 °C are tolerated

    Explanation

    The permitted error is ±0.5 °C (±1 °F), so a 1.0 °C deviation in an ice bath shows the thermometer is out of tolerance. It must be taken out of service until it is recalibrated or replaced.

  36. Question 36Temperature of Freshly Mixed Concrete

    A field thermometer is dropped on the pavement but looks undamaged. Before it is used again it must be:

    1. Verified against an ice bath or a reference thermometer Correct answer.
    2. Shaken down and returned to its protective case
    3. Compared with the reading of a second field thermometer
    4. Replaced, because a dropped thermometer can never be reused

    Explanation

    Any thermometer that has been dropped, or whose accuracy is in doubt, must be verified against a reference thermometer or an ice bath before further use. Verification, not appearance, decides whether it can stay in service.

  37. Question 37Temperature of Freshly Mixed Concrete

    How often does the temperature test method require the temperature of fresh concrete to be measured?

    1. The method sets no frequency; the specifications do Correct answer.
    2. Once for every 50 m³ (50 yd³) of concrete produced
    3. Once per day, at the start of the first truck of the day
    4. Each time the ambient air temperature changes by 5 °C (10 °F)

    Explanation

    The test method describes how to measure and report the temperature but does not establish how often it is done. Sampling frequency comes from the project specifications or the quality control plan.

  38. Question 38Temperature of Freshly Mixed Concrete

    When a sample is taken from a truck mixer for a temperature measurement, the concrete should be obtained:

    1. From the last portion of the discharge, after full mixing
    2. From the first portion of the discharge, which is warmest
    3. From the middle portion of the discharge Correct answer.
    4. From the drum after the truck has been stopped for 10 minutes

    Explanation

    Standard sampling practice requires the sample to come from the middle portion of the discharge. The first and last portions are not representative of the batch.

  39. Question 39Temperature of Freshly Mixed Concrete

    After the thermometer has been in the concrete for the required time, the technician should:

    1. Read it while the sensing portion stays immersed Correct answer.
    2. Withdraw it slowly and read it before the column begins to fall
    3. Lift it out quickly and read it at eye level against the sky
    4. Wipe the stem clean, then read the temperature to the nearest 1 °C

    Explanation

    The reading is taken with the sensing portion still in the concrete, because removing it exposes the sensor to air and the indicated value changes. The reading is recorded to the nearest 0.5 °C (1 °F).

  40. Question 40Temperature of Freshly Mixed Concrete

    Unless the project specifications state otherwise, the minimum temperature of concrete at the time of placement is:

    1. 5 °C (40 °F)
    2. 10 °C (50 °F) Correct answer.
    3. 0 °C (32 °F)
    4. 21 °C (70 °F)

    Explanation

    The general minimum placement temperature is 10 °C (50 °F) unless the specifications set a different value. Colder concrete gains strength slowly and is vulnerable to early freezing.

  41. Question 41Temperature of Freshly Mixed Concrete

    A sample sits in a wheelbarrow in direct sunlight for several minutes before the temperature is taken, and the reading is 3 °F higher than the previous truck. The most likely reason is:

    1. The thermometer was immersed too deeply in the sample
    2. The concrete was over-mixed in the drum before discharge
    3. The small sample absorbed heat from the sun and warm air Correct answer.
    4. The sensing portion was still equilibrating with the concrete

    Explanation

    A wheelbarrow sample has little thermal mass, so direct sun and hot air can raise its temperature within minutes. Samples should be protected from the sun and tested promptly.

  42. Question 42Temperature of Freshly Mixed Concrete

    Which statement about using a digital thermometer for this test is correct?

    1. A digital instrument must be recalibrated after every test
    2. It may be used if its accuracy meets the requirement Correct answer.
    3. Digital instruments are not permitted by the test method
    4. A digital instrument may be used only below 20 °C (68 °F)

    Explanation

    The test method does not restrict the type of instrument; any thermometer that meets the range, readability, and accuracy requirements and has been verified may be used. Digital thermometers are common in field work.

  43. Question 43Temperature of Freshly Mixed Concrete

    A truck arrives and the concrete temperature is 97 °F (36 °C). With respect to the general maximum placement temperature, the technician should:

    1. Record the reading and test the next truck instead
    2. Accept the load, since the limit applies only after placement
    3. Report that the concrete exceeds the 95 °F (35 °C) limit Correct answer.
    4. Wait 30 minutes for the concrete to cool before placing

    Explanation

    The general maximum is 95 °F (35 °C) at the time of placement, so 97 °F is a nonconformance that must be reported. The technician does not have authority to accept out-of-limit concrete.

  44. Question 44Temperature of Freshly Mixed Concrete

    Of the following, which normally has the greatest influence on the temperature of a freshly mixed batch?

    1. The temperature of the cement
    2. The temperature of the entrained air
    3. The temperature of the admixtures
    4. The temperature of the aggregates Correct answer.

    Explanation

    Aggregates make up most of the mass of a concrete mixture and their specific heat is comparable to that of the paste, so their temperature dominates the batch temperature. Cement, water, and admixtures are smaller fractions.

  45. Question 45Temperature of Freshly Mixed Concrete

    For the temperature reading to be valid, the sample must:

    1. Be held in a metal container fitted with a lid
    2. Be at least 24 hours old before measuring
    3. Fill the container almost to the rim before reading
    4. Be deep enough to surround the sensor on all sides Correct answer.

    Explanation

    The sample has to be deep enough that concrete surrounds the sensing portion on all sides; otherwise the reading is influenced by the container and the surrounding air. Container material and fill height are not the controlling requirements.

  46. Question 46Temperature of Freshly Mixed Concrete

    The temperature of a batch should be measured:

    1. As soon as the coarse aggregate enters the drum
    2. Before any water is added to the drum
    3. After all ingredients have been mixed together Correct answer.
    4. While the cement is being added at the plant

    Explanation

    The temperature is measured on concrete, meaning after all ingredients are in the drum and mixing is complete. Partial batches or dry materials do not represent the concrete being delivered.

  47. Question 47Temperature of Freshly Mixed Concrete

    Ice is more effective than an equal mass of water at the same temperature for cooling concrete because:

    1. Ice dissolves in the mix and lowers the water-cement ratio
    2. Ice floats and spreads more evenly through the drum
    3. Melting ice absorbs latent heat in addition to warming Correct answer.
    4. Ice has a much higher specific heat than liquid water

    Explanation

    Melting ice absorbs a large amount of latent heat, roughly 144 Btu per pound, on top of the sensible heat gained as it warms to the concrete temperature. That is why a kilogram of ice removes far more heat than a kilogram of cold water.

  48. Question 48Temperature of Freshly Mixed Concrete

    A 1.2 m (4 ft) thick foundation mat is placed at 80 °F (27 °C). Why may the highest temperature the concrete reaches occur hours after placement?

    1. Because the ambient air is usually warmer in the afternoon
    2. Because the aggregate continues to absorb water and warm up
    3. Because the thermometer used in the field is not accurate enough
    4. Because hydrating cement releases heat that builds up in the mass Correct answer.

    Explanation

    Cement hydration is exothermic, and in a thick section the heat cannot escape quickly, so the interior temperature climbs for hours after placement. The peak internal temperature can be well above the temperature measured at discharge.

  49. Question 49Temperature of Freshly Mixed Concrete

    A thermometer reads 0.4 °C (33 °F) in a properly prepared ice-water bath. How should the technician proceed?

    1. Accept it only if the same error appears in boiling water
    2. Reject it; any deviation from 0 °C is a failure
    3. Accept it; the reading is within ±0.5 °C of the ice point Correct answer.
    4. Reject it; error must be under 0.1 °C to be acceptable

    Explanation

    An ice-water bath is at 0 °C (32 °F), and an error of 0.4 °C is inside the ±0.5 °C (±1 °F) tolerance, so the thermometer may be used. It is not necessary for the instrument to read exactly zero.

  50. Question 50Temperature of Freshly Mixed Concrete

    A project specification sets a maximum concrete temperature of 90 °F, while the general industry limit is 95 °F. Which limit applies, and why?

    1. 95 °F, because the specification limit is only a suggestion
    2. 95 °F, because the general limit governs all concrete placement
    3. Either limit, since both are recognized industry standards
    4. 90 °F, because the more restrictive project limit governs Correct answer.

    Explanation

    Both documents apply, and where the specification is stricter, the stricter requirement controls. The project specification may tighten the general limit but may not relax it.

  51. Question 51Temperature of Freshly Mixed Concrete

    Compared with cool concrete, concrete that is mixed and placed at a high temperature typically shows:

    1. Faster slump loss and higher entrained air content
    2. Slower slump loss and the same entrained air content
    3. Faster slump loss and lower entrained air content Correct answer.
    4. Slower slump loss and higher entrained air content

    Explanation

    Higher temperature accelerates hydration and evaporation, so slump is lost faster and the mixture holds less entrained air. That is why hot-weather concreting requires faster placement and closer air-content control.

  52. Question 52Temperature of Freshly Mixed Concrete

    Under the standard field test method, what is the minimum period the thermometer must remain in the fresh concrete before a reading is taken, if the reading has not already become constant?

    1. 5 minutes
    2. 1 minute
    3. 2 minutes Correct answer.
    4. 30 seconds

    Explanation

    The sensing portion is fully immersed and left undisturbed for at least 2 minutes or until the reading stabilizes, whichever occurs first. This allows the thermometer to reach thermal equilibrium with the concrete so the recorded value represents the concrete rather than the thermometer's initial temperature.

  53. Question 53Slump of Hydraulic Cement Concrete

    What are the internal dimensions of the standard slump cone used in field testing?

    1. 4 in. top diameter, 8 in. bottom diameter, 12 in. height Correct answer.
    2. 4 in. top diameter, 8 in. bottom diameter, 6 in. height
    3. 6 in. top diameter, 12 in. bottom diameter, 12 in. height
    4. 8 in. top diameter, 4 in. bottom diameter, 12 in. height

    Explanation

    The slump mold is a frustum of a cone with a 4 in. (100 mm) top opening, an 8 in. (200 mm) bottom opening, and a 12 in. (300 mm) height. The smaller opening is placed upward during filling.

  54. Question 54Slump of Hydraulic Cement Concrete

    Which tamping rod is specified for the slump test?

    1. 5/8 in. diameter by 24 in. long, rounded ends Correct answer.
    2. 5/8 in. diameter by 12 in. long, flat ends
    3. 1/2 in. diameter by 24 in. long, rounded ends
    4. 3/4 in. diameter by 36 in. long, rounded ends

    Explanation

    The standard rod is 5/8 in. (16 mm) in diameter and approximately 24 in. (600 mm) long. It has rounded ends so rodding does not tear the concrete.

  55. Question 55Slump of Hydraulic Cement Concrete

    Into how many layers is the slump cone filled?

    1. Five layers
    2. Two layers
    3. Four layers
    4. Three layers Correct answer.

    Explanation

    The mold is filled in three approximately equal-volume layers. Each layer is rodded before the next is added.

  56. Question 56Slump of Hydraulic Cement Concrete

    How many strokes of the tamping rod are required for each layer in the slump test?

    1. 15
    2. 30
    3. 25 Correct answer.
    4. 20

    Explanation

    Each of the three layers receives 25 strokes. The strokes are distributed uniformly over the layer.

  57. Question 57Slump of Hydraulic Cement Concrete

    How should the 25 rod strokes be distributed within each layer?

    1. Uniformly across the layer Correct answer.
    2. Along the inside edge of the mold only
    3. In a tight spiral around the mold wall
    4. At the center of the layer only

    Explanation

    Strokes are distributed uniformly over the cross section so the concrete is consolidated evenly. Concentrating strokes at the edge or center can leave voids.

  58. Question 58Slump of Hydraulic Cement Concrete

    After striking off the top, how should the slump mold be removed?

    1. Tilt it forward quickly while lifting
    2. Raise it vertically in 5 ± 2 seconds Correct answer.
    3. Raise it vertically over about 30 seconds
    4. Slide it sideways off the concrete

    Explanation

    The mold is lifted straight up in 5 ± 2 seconds. Any tilting or sideways motion can distort the slumped shape and change the reading.

  59. Question 59Slump of Hydraulic Cement Concrete

    Where is the slump measured after the mold is removed?

    1. At the average of the four sides
    2. At the edge nearest the tester
    3. At the highest point of the slumped concrete
    4. At the original center of the top Correct answer.

    Explanation

    Slump is measured at the displaced original center of the top surface, not at a high point or edge. The reading is the vertical distance from the mold top to that point.

  60. Question 60Slump of Hydraulic Cement Concrete

    To what nearest increment is the slump measured in the standard field test?

    1. 1/2 in. (13 mm)
    2. 1/4 in. (5 mm) Correct answer.
    3. 1/16 in. (1 mm)
    4. 1/8 in. (3 mm)

    Explanation

    The slump is measured to the nearest 1/4 in. (5 mm). Reporting a more precise value implies accuracy the test does not provide.

  61. Question 61Slump of Hydraulic Cement Concrete

    What is required of the surface on which the slump mold is placed?

    1. It is soft, level, and absorbent
    2. It is flexible, level, and nonabsorbent
    3. It is rigid, sloped, and absorbent
    4. It is rigid, level, and nonabsorbent Correct answer.

    Explanation

    The mold must rest on a rigid, level, nonabsorbent surface that will not settle or absorb water. This keeps the mold stable and the test repeatable.

  62. Question 62Slump of Hydraulic Cement Concrete

    How is the slump mold prepared before concrete is placed in it?

    1. It is heated to drive off moisture
    2. Mold and base are dampened Correct answer.
    3. It is coated with release oil
    4. It is lined with absorbent paper

    Explanation

    The mold and its base are dampened before use so they do not absorb water from the concrete. Excess water should be poured off.

  63. Question 63Slump of Hydraulic Cement Concrete

    How is the top layer finished before the mold is lifted?

    1. It is mounded well above the mold rim
    2. It is struck off level with the rim Correct answer.
    3. It is troweled to a smooth, sealed surface
    4. It is left rough and uncompacted

    Explanation

    The top layer is struck off level with the top of the mold using the tamping rod. Mounding, troweling, or leaving the surface rough changes the standard specimen.

  64. Question 64Slump of Hydraulic Cement Concrete

    Why does the tester step on the foot pieces of the slump mold during filling?

    1. To keep the mold from moving Correct answer.
    2. To tilt the mold toward the tester
    3. To compact the concrete at the bottom
    4. To raise the mold slightly off the base

    Explanation

    Stepping on the foot pieces holds the mold firmly against the base while it is filled and rodded. A mold that lifts or shifts can create voids and invalidate the test.

  65. Question 65Slump of Hydraulic Cement Concrete

    The standard slump test is applicable to concrete whose nominal maximum coarse aggregate size does not exceed which value?

    1. 1-1/2 in. (37.5 mm) Correct answer.
    2. 2 in. (50 mm)
    3. 3 in. (75 mm)
    4. 2-1/2 in. (63 mm)

    Explanation

    The test is limited to concrete with coarse aggregate no larger than 1-1/2 in. (37.5 mm). Larger aggregate is too large relative to the 8 in. cone for a representative specimen.

  66. Question 66Slump of Hydraulic Cement Concrete

    What does a shear slump generally indicate about the concrete?

    1. The specimen sheared to one side Correct answer.
    2. The concrete set too quickly in the mold
    3. The concrete has an unusually high cement content
    4. The mold was lifted too slowly

    Explanation

    A shear slump means part of the specimen has slid sideways instead of settling as a symmetrical mass. This often indicates a mix with low cohesion.

  67. Question 67Slump of Hydraulic Cement Concrete

    A collapse slump is most characteristic of which condition?

    1. A mixture with excessive coarse aggregate
    2. A mixture that has false set
    3. A very dry, low-slump mixture
    4. A very flowable, high-slump mix Correct answer.

    Explanation

    A collapse slump occurs when the specimen falls outward and loses its conical shape. It is typical of very wet, highly flowable concrete, and the numerical slump may be of little value.

  68. Question 68Slump of Hydraulic Cement Concrete

    The slump value is defined as the vertical difference between which two elevations?

    1. The original base and the final top of the concrete
    2. Mold top and the displaced original center Correct answer.
    3. The top and bottom of the slump mold
    4. The highest and lowest points of the slumped specimen

    Explanation

    Slump is the vertical distance from the top of the mold to the displaced original center of the top surface. It is not a spread measurement or a difference between high and low points.

  69. Question 69Slump of Hydraulic Cement Concrete

    What does a slump test primarily measure?

    1. Workability for all placement methods
    2. Compressive strength of the concrete
    3. Air content of the concrete
    4. Consistency of fresh concrete Correct answer.

    Explanation

    Slump is an empirical measure of consistency, or how wet and flowable the mixture is. Workability is broader and depends on the placement method and other mixture properties.

  70. Question 70Slump of Hydraulic Cement Concrete

    What time limit applies to completing the slump test after the sample is obtained?

    1. Within 10 minutes
    2. Within 1 hour
    3. Within 30 seconds
    4. Within 2-1/2 minutes Correct answer.

    Explanation

    The standard requires the slump test to be completed within 2-1/2 minutes after obtaining the sample. Delay allows the concrete to stiffen or segregate.

  71. Question 71Slump of Hydraulic Cement Concrete

    If the first slump test results in a shear slump, what should the tester do?

    1. Add water and repeat the test
    2. Trowel the specimen and measure again
    3. Record the shear value as the slump
    4. Obtain another sample and repeat the test Correct answer.

    Explanation

    A sheared specimen does not provide a valid slump reading. The tester should repeat the test on another portion of the sample; repeated shear may be reported as a lack of cohesion.

  72. Question 72Slump of Hydraulic Cement Concrete

    Why is the slump test of limited value for a very dry, no-slump mixture?

    1. The tamping rod is too small for the aggregate
    2. It may not settle enough to read Correct answer.
    3. The cone cannot be filled in three layers
    4. The mold absorbs water from the dry mix

    Explanation

    A very dry mixture may barely move or may crumble when the mold is lifted. The test then does not distinguish small differences in consistency well.

  73. Question 73Slump of Hydraulic Cement Concrete

    What describes a true slump?

    1. One side slides away from the rest
    2. It remains at full mold height
    3. It falls completely outward into a flat pile
    4. It settles evenly without shear or collapse Correct answer.

    Explanation

    A true slump is a roughly symmetrical settlement of the concrete cone. Shear and collapse are different modes that can make the measurement invalid or unrepresentative.

  74. Question 74Slump of Hydraulic Cement Concrete

    How is the slump mold oriented when concrete is placed?

    1. Smaller opening up, larger opening down Correct answer.
    2. Larger opening up, smaller opening down
    3. Either opening may be up
    4. Smaller opening down, larger opening up

    Explanation

    The 4 in. opening is at the top and the 8 in. opening rests on the base. Reversing the cone changes the volume and makes the test nonstandard.

  75. Question 75Slump of Hydraulic Cement Concrete

    When rodding the second and third layers, how deep should the rod penetrate?

    1. To the bottom of the mold every time
    2. Only the top half of the current layer
    3. Through the layer into the one below Correct answer.
    4. Just to the top of the layer below

    Explanation

    Upper layers are rodded through their full depth and about 1 in. into the layer below. This integrates the layers and prevents a weak horizontal plane.

  76. Question 76Slump of Hydraulic Cement Concrete

    How is the first layer rodded in the slump test?

    1. With 15 strokes around the mold edge
    2. With 25 strokes that stop at mid-depth
    3. With 25 strokes that penetrate only the top inch
    4. With 25 strokes through the full layer Correct answer.

    Explanation

    The bottom layer receives 25 uniformly distributed strokes, and the rod passes through the full depth of that layer. Partial-depth rodding leaves unconsolidated concrete at the base.

  77. Question 77Slump of Hydraulic Cement Concrete

    Two slump tests on the same sample give 3 in. and 5 in. What is the most appropriate interpretation?

    1. The higher value is always the correct slump
    2. Both results are acceptable because slump is approximate
    3. The difference is large enough to require a check Correct answer.
    4. The lower value is always the correct slump

    Explanation

    A 2 in. difference is larger than the normal single-operator variation for this test. The tester should review the procedure and retest before accepting either result.

  78. Question 78Slump of Hydraulic Cement Concrete

    A tester fills a slump mold in three equal layers. Within each layer, how should the rodding strokes be positioned?

    1. Concentrated near the center to drive out entrapped air
    2. Around the perimeter only, leaving the middle undisturbed
    3. Uniformly over the whole cross section, rod held vertical Correct answer.
    4. In a single line along one diameter of the mold

    Explanation

    Each layer must be rodded uniformly over its entire cross section, with the rod held vertically, so that every part of the layer receives the same consolidation effort. Strokes that are bunched in one region leave unrodded pockets elsewhere in the layer, which can produce a honeycombed mass or an unrepresentative result. Working across the section also keeps the energy input consistent from layer to layer.

  79. Question 79Density (Unit Weight), Yield, and Air Content (Gravimetric) of Concrete

    In ASTM C138, what does the unit weight (density) of concrete represent?

    1. The mass of cement per unit volume of concrete
    2. The volume of concrete per unit mass
    3. The volume of air voids per unit volume of concrete
    4. The mass of concrete per unit volume Correct answer.

    Explanation

    Unit weight, or density, is defined as the mass of a given volume of concrete, typically expressed in lb/ft³ or kg/m³. It is determined by dividing the mass of concrete in a calibrated measure by the measure's volume. This value is used to calculate yield and, together with theoretical density, gravimetric air content.

  80. Question 80Density (Unit Weight), Yield, and Air Content (Gravimetric) of Concrete

    How is the yield of a concrete batch calculated from the unit weight and the total batch mass?

    1. Yield = volume of measure ÷ unit weight
    2. Yield = unit weight ÷ total batch mass
    3. Yield = total batch mass ÷ unit weight Correct answer.
    4. Yield = total batch mass × unit weight

    Explanation

    Yield is the volume of concrete produced by a batch. ASTM C138 calculates it by dividing the total mass of all materials batched by the measured unit weight (density) of the concrete. This gives the batch volume in the same units as the density.

  81. Question 81Density (Unit Weight), Yield, and Air Content (Gravimetric) of Concrete

    What does a relative yield of 0.96 indicate for a concrete batch?

    1. The batch produced 96% air content
    2. The batch unit weight is 96% of the theoretical density
    3. The batch produced 4% less volume than the design volume Correct answer.
    4. The batch produced 4% more volume than the design volume

    Explanation

    Relative yield is the actual yield divided by the design batch volume. A value of 0.96 means the batch produced only 96% of the intended volume, which is 4% less volume than design. This condition is described as under-yielding.

  82. Question 82Density (Unit Weight), Yield, and Air Content (Gravimetric) of Concrete

    Which expression gives the air content of concrete by the gravimetric method?

    1. A = (T − D) ÷ T × 100 Correct answer.
    2. A = (D ÷ T) × 100
    3. A = (T − D) ÷ D × 100
    4. A = (D − T) ÷ D × 100

    Explanation

    In ASTM C138, the gravimetric air content is the difference between the theoretical air-free density T and the measured density D, divided by T and multiplied by 100. This expresses the air volume as a percentage of the theoretical volume. The theoretical density represents the concrete with zero air.

  83. Question 83Density (Unit Weight), Yield, and Air Content (Gravimetric) of Concrete

    When consolidating concrete in the unit weight measure by rodding, how many approximately equal layers are used?

    1. Five
    2. Three Correct answer.
    3. Two
    4. Four

    Explanation

    ASTM C138 requires filling the measure in three approximately equal layers when consolidating by rodding or vibration. Each layer is consolidated before the next is added. This ensures uniform density throughout the measure.

  84. Question 84Density (Unit Weight), Yield, and Air Content (Gravimetric) of Concrete

    At a minimum, how often must the volume of a unit weight measure be calibrated?

    1. Every week
    2. Every two years
    3. At least annually Correct answer.
    4. Only when first purchased

    Explanation

    ASTM C138 requires calibration of the measure's volume at least annually, or whenever there is reason to question its accuracy. Calibration is typically performed by filling the measure with water and determining its volume from the mass of the water at a known temperature.

  85. Question 85Density (Unit Weight), Yield, and Air Content (Gravimetric) of Concrete

    After consolidating the final layer of concrete in the measure, what is the correct procedure for finishing the top surface?

    1. Strike off the surface with a straightedge and cover with a plate Correct answer.
    2. Trowel the surface to a smooth finish and remove the rim
    3. Leave the surface mounded above the rim
    4. Tap the sides of the measure until the surface settles

    Explanation

    ASTM C138 requires striking off the top surface with a straightedge to remove excess concrete and produce a flat surface flush with the rim. The outside of the measure is then cleaned, and the mass is determined. Covering the measure is not part of the density procedure.

  86. Question 86Density (Unit Weight), Yield, and Air Content (Gravimetric) of Concrete

    For concrete with a slump less than 25 mm (1 in.), which consolidation method does ASTM C138 require?

    1. Internal vibration Correct answer.
    2. Rodding only
    3. Rodding or vibration, at the technician's choice
    4. Tapping the measure with a mallet

    Explanation

    ASTM C138 specifies internal vibration for concrete with slump less than 25 mm (1 in.). For slump between 25 and 75 mm, either rodding or vibration may be used; for slump greater than 75 mm, rodding is required.

  87. Question 87Density (Unit Weight), Yield, and Air Content (Gravimetric) of Concrete

    A concrete mixture has a theoretical air-free density of 150.0 lb/ft³. The measured unit weight is 144.0 lb/ft³. What is the gravimetric air content?

    1. 6.0%
    2. 4.2%
    3. 4.0% Correct answer.
    4. 96.0%

    Explanation

    Air content = (T − D) ÷ T × 100 = (150.0 − 144.0) ÷ 150.0 × 100 = 6.0 ÷ 150.0 × 100 = 4.0%. The theoretical density represents the concrete with zero air, so the density difference is attributed to air voids.

  88. Question 88Density (Unit Weight), Yield, and Air Content (Gravimetric) of Concrete

    A batch contains 3,600 lb of total materials. The measured unit weight is 148.0 lb/ft³. What is the yield of the batch?

    1. 532,800 ft³
    2. 24.3 ft³ Correct answer.
    3. 0.041 ft³
    4. 148 ft³

    Explanation

    Yield = total batch mass ÷ unit weight = 3,600 lb ÷ 148.0 lb/ft³ = 24.3 ft³. This is the volume of concrete produced by the batch. The yield is used with batch proportions to determine cement content per unit volume.

  89. Question 89Density (Unit Weight), Yield, and Air Content (Gravimetric) of Concrete

    A batch has a yield of 24.3 ft³ and contains 600 lb of cement. What is the cement content per cubic yard?

    1. 24.7 lb/yd³
    2. 666.7 lb/yd³ Correct answer.
    3. 22.2 lb/yd³
    4. 600 lb/yd³

    Explanation

    Cement content = mass of cement ÷ yield = 600 lb ÷ 24.3 ft³ = 24.69 lb/ft³. Since 1 yd³ = 27 ft³, multiply by 27: 24.69 × 27 = 666.7 lb/yd³. The under-yield has increased the cement factor above the intended 600 lb/yd³.

  90. Question 90Density (Unit Weight), Yield, and Air Content (Gravimetric) of Concrete

    The theoretical air-free density of concrete used in the gravimetric air content method is calculated from which quantities?

    1. The measured unit weight and the volume of the measure
    2. The total batch mass and the measured air content
    3. The mass of concrete in the measure and the batch mass
    4. The total batch mass and the sum of the absolute volumes of all ingredients Correct answer.

    Explanation

    Theoretical density T = total mass of all materials batched ÷ total absolute volume of those materials. Absolute volumes are computed from each ingredient's mass and specific gravity. This represents the density the concrete would have if it contained no air.

  91. Question 91Density (Unit Weight), Yield, and Air Content (Gravimetric) of Concrete

    What is the absolute volume of 500 lb of cement with a specific gravity of 3.15? Use 62.4 lb/ft³ for the density of water.

    1. 2.54 ft³ Correct answer.
    2. 0.39 ft³
    3. 8.01 ft³
    4. 31,200 ft³

    Explanation

    Absolute volume = mass ÷ (specific gravity × density of water) = 500 ÷ (3.15 × 62.4) = 500 ÷ 196.56 = 2.54 ft³. This volume is used in computing the theoretical density of the concrete.

  92. Question 92Density (Unit Weight), Yield, and Air Content (Gravimetric) of Concrete

    A batch has a design volume of 27.0 ft³ and a calculated yield of 28.1 ft³. What is the relative yield, and what does it indicate?

    1. 1.041; the batch under-yielded and the cement factor increased
    2. 0.961; the batch over-yielded and the cement factor decreased
    3. 1.041; the batch over-yielded and the cement factor decreased Correct answer.
    4. 0.961; the batch under-yielded and the cement factor increased

    Explanation

    Relative yield = actual yield ÷ design volume = 28.1 ÷ 27.0 = 1.041. A value greater than 1.0 means the batch produced more volume than design, which is over-yielding. Because the cement mass is spread over more volume, the cement factor decreases.

  93. Question 93Density (Unit Weight), Yield, and Air Content (Gravimetric) of Concrete

    A batch contains 540 lb of cement and 270 lb of water. What is the water-cement ratio?

    1. 0.50 Correct answer.
    2. 0.54
    3. 0.27
    4. 2.00

    Explanation

    Water-cement ratio = mass of water ÷ mass of cement = 270 ÷ 540 = 0.50. This ratio is based on batch masses and is not directly changed by yield, provided all materials are proportionally adjusted.

  94. Question 94Density (Unit Weight), Yield, and Air Content (Gravimetric) of Concrete

    When rodding a 0.5 ft³ (14 L) unit weight measure, how many strokes per layer does ASTM C138 require?

    1. 25 Correct answer.
    2. 15
    3. 10
    4. 50

    Explanation

    ASTM C138 specifies 25 strokes per layer for a 0.5 ft³ (14 L) measure and 50 strokes per layer for a 1.0 ft³ (28 L) measure. The strokes are distributed uniformly over the cross section of each layer.

  95. Question 95Density (Unit Weight), Yield, and Air Content (Gravimetric) of Concrete

    If all other factors remain constant, what happens to the measured unit weight of concrete as its air content increases?

    1. The unit weight decreases Correct answer.
    2. The unit weight increases
    3. The unit weight remains unchanged
    4. The unit weight first increases, then decreases

    Explanation

    Air voids have negligible mass, so replacing solid concrete with air reduces the mass per unit volume. Therefore, higher air content lowers the measured unit weight. This relationship is the basis for the gravimetric air content method.

  96. Question 96Density (Unit Weight), Yield, and Air Content (Gravimetric) of Concrete

    For which type of concrete is the gravimetric air content method of ASTM C138 not applicable?

    1. Concrete with a slump greater than 75 mm
    2. Concrete with a maximum aggregate size of 1 in.
    3. Air-entrained normal-weight concrete
    4. Concrete containing lightweight aggregate Correct answer.

    Explanation

    The gravimetric method assumes that the measured density differs from the theoretical density only because of air voids. Lightweight or highly porous aggregates contain voids within the particles, which distort the density and make the computed air content unreliable. The method is therefore not applicable to such concrete.

  97. Question 97Density (Unit Weight), Yield, and Air Content (Gravimetric) of Concrete

    When determining the mass of concrete in a unit weight measure, ASTM C138 requires the mass to be recorded to the nearest:

    1. 0.1 lb (0.05 kg) or 0.3% of the mass, whichever is greater Correct answer.
    2. 5 lb (2 kg)
    3. 1 lb (0.5 kg)
    4. 0.01 lb (0.005 kg)

    Explanation

    ASTM C138 requires the mass of concrete in the measure to be determined to the nearest 0.1 lb (0.05 kg) or 0.3% of the mass, whichever is greater. This precision ensures that the calculated density and yield are not limited by weighing error. For typical measure masses, the 0.1 lb criterion usually governs.

  98. Question 98Density (Unit Weight), Yield, and Air Content (Gravimetric) of Concrete

    A batch consistently over-yields by 5%. Which adjustment is most appropriate for the next batch if the same design volume is required?

    1. Increase the cement content by 5%
    2. Increase the water content by 5%
    3. Increase all batch quantities by 5%
    4. Reduce the batch quantities proportionally to produce the design volume Correct answer.

    Explanation

    Over-yield means the batch produces more volume than intended, so the cement factor is lower than design. To produce the intended volume with the correct cement content, the batch masses should be reduced proportionally or the mix proportions adjusted. Increasing materials would worsen the over-yield.

  99. Question 99Density (Unit Weight), Yield, and Air Content (Gravimetric) of Concrete

    A batch has a total mass of 4,080 lb and a total absolute volume of 27.2 ft³. The measured unit weight is 142.5 lb/ft³. What is the gravimetric air content?

    1. 95.0%
    2. 4.8%
    3. 5.0% Correct answer.
    4. 5.3%

    Explanation

    Theoretical density = 4,080 ÷ 27.2 = 150.0 lb/ft³. Air content = (150.0 − 142.5) ÷ 150.0 × 100 = 7.5 ÷ 150.0 × 100 = 5.0%. The theoretical density is based on the absolute volumes of all ingredients.

  100. Question 100Density (Unit Weight), Yield, and Air Content (Gravimetric) of Concrete

    Why is the gravimetric method generally less suitable than the pressure method for routine field air content testing of normal-weight concrete?

    1. The gravimetric method cannot detect entrained air
    2. The gravimetric method requires accurate batch masses and specific gravities for all ingredients Correct answer.
    3. The gravimetric method requires a pressurized vessel
    4. The gravimetric method is only valid for concrete with slump less than 25 mm

    Explanation

    The gravimetric method calculates air content from the difference between theoretical and measured density, so it depends on knowing the batch masses and specific gravities of all ingredients. In the field, these data may be uncertain or unavailable, whereas the pressure method directly measures air content with a meter. The gravimetric method is also not applicable to lightweight aggregate concrete.

  101. Question 101Density (Unit Weight), Yield, and Air Content (Gravimetric) of Concrete

    A 0.25 ft³ measure filled with concrete has a total mass of 37.5 lb. The empty measure weighs 2.5 lb. What is the unit weight of the concrete?

    1. 148.0 lb/ft³
    2. 150.0 lb/ft³
    3. 140.0 lb/ft³ Correct answer.
    4. 160.0 lb/ft³

    Explanation

    Mass of concrete = 37.5 − 2.5 = 35.0 lb. Unit weight = 35.0 ÷ 0.25 = 140.0 lb/ft³. The empty measure mass must always be subtracted before dividing by the measure volume.

  102. Question 102Density (Unit Weight), Yield, and Air Content (Gravimetric) of Concrete

    Which condition would make a gravimetric air content result unreliable even for normal-weight concrete?

    1. The concrete is air-entrained
    2. The slump is 100 mm (4 in.)
    3. The batch masses are estimated rather than measured Correct answer.
    4. The measure volume is 0.5 ft³ (14 L)

    Explanation

    The gravimetric method computes air content from the theoretical density, which depends on the actual masses and specific gravities of all ingredients. If batch masses are estimated, the theoretical density is inaccurate, and the calculated air content will be unreliable. Air entrainment, slump, and a standard measure size do not by themselves invalidate the method.

  103. Question 103Density (Unit Weight), Yield, and Air Content (Gravimetric) of Concrete

    A concrete batch is found to have a higher air content than design while the batch masses remain as designed. What is the most likely effect on yield and cement factor?

    1. Yield increases and cement factor decreases Correct answer.
    2. Yield decreases and cement factor increases
    3. Yield and cement factor both remain unchanged
    4. Yield increases and cement factor increases

    Explanation

    Higher air content lowers the unit weight, so the same total batch mass occupies more volume, which increases yield. Because the cement mass is unchanged but spread over a larger volume, the cement content per cubic yard, or cement factor, decreases. This is why air content must be controlled to maintain specified cement content.

  104. Question 104Density (Unit Weight), Yield, and Air Content (Gravimetric) of Concrete

    A gravimetric air content calculation yields a negative value. What is the most appropriate interpretation?

    1. The result is valid and should be reported as a negative air content.
    2. Air content is zero, so report 0.0% for the batch.
    3. The test has an error in measured unit weight or theoretical density. Correct answer.
    4. The concrete contains only entrapped air and no entrained air.

    Explanation

    A negative calculated air content has no physical meaning because air content cannot be less than zero. It occurs when the measured unit weight exceeds the theoretical air-free density used in the calculation, indicating an error in the measured mass, the measure volume, or the theoretical density. The result should be investigated and corrected rather than reported as a valid air content.

  105. Question 105Air Content of Freshly Mixed Concrete by the Pressure Method

    The pressure method determines the air content of fresh concrete by measuring which quantity?

    1. The time for a fixed volume of water to pass through the sample
    2. The weight of water displaced by the sample
    3. The volume change produced by an applied pressure Correct answer.
    4. The electrical resistance between probes in the concrete

    Explanation

    Air is far more compressible than water, cement paste solids, or dense aggregate. When a known pressure is applied, the volume change of the concrete is essentially all due to compression of its air voids, so the gauge can be graduated directly in percent air.

  106. Question 106Air Content of Freshly Mixed Concrete by the Pressure Method

    What must the operator do before removing the lid of the air meter after a test is complete?

    1. Open the water inlet valve and add water to the bowl
    2. Loosen the clamps while the bowl is still under pressure
    3. Strike off the concrete again with the strike-off plate
    4. Release the pressure, then check the gauge reads zero Correct answer.

    Explanation

    Trapped pressure can blow the lid off or spray concrete when the clamps are released, so the pressure must be vented through the valve first. The needle should return to zero, confirming the vessel is at atmospheric pressure before the lid is handled.

  107. Question 107Air Content of Freshly Mixed Concrete by the Pressure Method

    The pressure method gives unreliable air contents for concrete made with which of the following?

    1. Crushed limestone coarse aggregate
    2. Air-entraining admixtures
    3. Highly porous lightweight aggregate Correct answer.
    4. Natural sand and gravel

    Explanation

    The method assumes the only compressible phase is the air in the paste. Porous aggregate contains air in its own voids, which compresses under the test pressure and makes the indicated air content meaningless. Such concrete must be tested by a volumetric method instead.

  108. Question 108Air Content of Freshly Mixed Concrete by the Pressure Method

    How is the concrete placed in the measuring bowl of the air meter?

    1. In four layers, each tamped with the lid
    2. In one continuous pour, then vibrated for 30 s
    3. In three roughly equal layers, each rodded Correct answer.
    4. In two layers, each rodded 10 times

    Explanation

    The bowl is filled in three equal layers, and each layer is rodded with the tamping rod so the concrete is uniformly consolidated. Consistent consolidation is needed so the bowl holds exactly the fixed volume the gauge is calibrated for.

  109. Question 109Air Content of Freshly Mixed Concrete by the Pressure Method

    Before any pressure is applied, the gauge of a properly maintained air meter should indicate:

    1. the expected air content of the concrete
    2. zero, with no pressure applied Correct answer.
    3. the calibration pressure stamped on the lid
    4. the aggregate correction factor

    Explanation

    The gauge is a pressure gauge graduated in percent air, so it must read zero when the vessel is at atmospheric pressure. A needle that does not return to zero indicates a damaged gauge or linkage, and the meter must not be used until it is corrected.

  110. Question 110Air Content of Freshly Mixed Concrete by the Pressure Method

    The air content reported by the pressure method represents:

    1. Total air, both entrained and entrapped Correct answer.
    2. Only air deliberately entrained by the admixture
    3. The volume of water displaced when the bowl is filled
    4. Only air trapped under coarse aggregate particles

    Explanation

    The meter responds to every compressible void in the sample, so both the small entrained bubbles and the larger accidental voids are counted. This is why good consolidation and a properly determined aggregate correction factor matter.

  111. Question 111Air Content of Freshly Mixed Concrete by the Pressure Method

    The air content obtained by the pressure method is normally expressed as:

    1. a pressure ratio with no units
    2. kilograms of air per cubic metre of concrete
    3. a percentage of the concrete volume Correct answer.
    4. litres of air per bag of cement

    Explanation

    Results are reported as the volume of air voids divided by the total volume of concrete, multiplied by 100. Specification limits for air content are also written on this volumetric basis.

  112. Question 112Air Content of Freshly Mixed Concrete by the Pressure Method

    An air meter reads 6.0% on the gauge, and the aggregate correction factor for the mix is 0.5%. What air content should be reported?

    1. 6.0%
    2. 5.5% Correct answer.
    3. 6.5%
    4. 3.0%

    Explanation

    The aggregate correction factor is subtracted from the gauge reading because part of the indicated air is air held in the aggregate. The reported air content is therefore 6.0 minus 0.5, or 5.5%.

  113. Question 113Air Content of Freshly Mixed Concrete by the Pressure Method

    How is the aggregate correction factor for a concrete mixture determined?

    1. By subtracting the gauge reading from the design air content
    2. By testing aggregates and water in the meter under pressure Correct answer.
    3. By compressing a hardened core in a hydraulic press
    4. By measuring the slump of the concrete and using a table

    Explanation

    A sample of the coarse and fine aggregate, in the same proportions as in the concrete, is placed in the bowl with water and pressurized. The resulting gauge reading is the correction factor, which is later subtracted from readings made on the actual concrete.

  114. Question 114Air Content of Freshly Mixed Concrete by the Pressure Method

    When should the aggregate correction factor be determined again?

    1. Never, because the gauge already accounts for the aggregates
    2. Only after the concrete fails a strength test
    3. Once at the start of a project, regardless of later material changes
    4. When the source or proportions of the aggregates change Correct answer.

    Explanation

    The factor depends on the porosity and grading of the specific aggregates and on their proportions in the mix. A change of source, or a significant change in proportions, invalidates the old factor and a new one must be established.

  115. Question 115Air Content of Freshly Mixed Concrete by the Pressure Method

    Why is the bowl tapped with a mallet after the pressure has been applied?

    1. To check the lid gasket for leaks while under pressure
    2. To break up local bridging so the gauge settles Correct answer.
    3. To compact the concrete further before the reading
    4. To bring the concrete to the calibration temperature

    Explanation

    Tapping helps release concrete that is bridging or clinging to the bowl wall, so the applied pressure reaches the whole sample. This lets the needle settle at a stable value that reflects the true volume change.

  116. Question 116Air Content of Freshly Mixed Concrete by the Pressure Method

    How is concrete that contains aggregate larger than 37.5 mm (1 1/2 in.) prepared for the pressure meter?

    1. Using a larger bowl and multiplying the reading by a factor
    2. The largest particles are picked out by hand before filling the bowl
    3. Wet-sieving the sample over a 37.5 mm sieve Correct answer.
    4. Testing as received and adding 1% to the gauge reading

    Explanation

    The meter and its calibration apply to concrete with aggregate no larger than 37.5 mm. Oversize concrete is wet-sieved and the passing portion is tested, which keeps the sample within the range the gauge was calibrated for.

  117. Question 117Air Content of Freshly Mixed Concrete by the Pressure Method

    During a test the needle keeps dropping after the pressure is applied. How should the result be treated?

    1. The reading may be used if 0.5% is added
    2. The reading is valid once the needle steadies
    3. The aggregate correction factor compensates for the leak
    4. The test is invalid and must be discarded Correct answer.

    Explanation

    A falling needle shows that air is escaping, so the pressure in the vessel is not the pressure the gauge calibration assumes. The test must be stopped, the seal and valves checked, and the test repeated on a fresh sample.

  118. Question 118Air Content of Freshly Mixed Concrete by the Pressure Method

    After consolidation, how should the concrete surface be finished before the lid is clamped on?

    1. Left roughly 10 mm below the rim to leave room for water
    2. Struck off flush and level with the rim Correct answer.
    3. Left about 6 mm above the rim so the lid compresses it
    4. Mounded in the centre and level at the edges

    Explanation

    The bowl must contain exactly its calibrated volume, so the surface is struck off flush with the rim and finished with a trowel. The flange is then wiped clean so the lid gasket seals properly.

  119. Question 119Air Content of Freshly Mixed Concrete by the Pressure Method

    In a Type B meter, water is introduced into the standpipe above the concrete so that:

    1. the concrete surface is kept from drying out during the test
    2. the gauge can be zeroed before the pressure is applied
    3. the aggregate correction factor can be measured directly
    4. the drop in the water level shows the volume change Correct answer.

    Explanation

    The water column acts as a visible indicator of volume change: when the sample compresses, the level in the sight tube falls. The pressure is adjusted until the level returns to its mark, and the gauge then gives the air content.

  120. Question 120Air Content of Freshly Mixed Concrete by the Pressure Method

    The calculation behind the pressure method treats the air in the concrete as:

    1. a rigid solid that does not change volume
    2. a vacuum that collapses under pressure
    3. an ideal gas compressed at constant temperature Correct answer.
    4. a compressible liquid that obeys Henry's law

    Explanation

    The gauge graduations are based on Boyle's law, with the air treated as an ideal gas and the temperature assumed constant during the short test. The water and solid constituents are treated as incompressible by comparison.

  121. Question 121Air Content of Freshly Mixed Concrete by the Pressure Method

    If the sample in the bowl is vibrated more than necessary, the indicated air content will tend to be:

    1. lower than the air content of the concrete as placed Correct answer.
    2. unchanged, because the meter measures only entrained air
    3. higher, because vibration creates new air bubbles
    4. higher than the air content of the concrete as placed

    Explanation

    Extra vibration drives off some of the large accidental voids that were present in the concrete as delivered. The tested sample is then no longer representative, and the meter reports less total air than the concrete actually contains.

  122. Question 122Air Content of Freshly Mixed Concrete by the Pressure Method

    What is the purpose of the calibration vessel supplied with an air meter?

    1. It measures the slump of the concrete before the test
    2. It determines the bulk specific gravity of the aggregate
    3. It stores the tamping rod and mallet between tests
    4. It checks the accuracy of the meter using a known volume Correct answer.

    Explanation

    The calibration vessel has a known, fixed volume and contains no compressible air, so pressurizing it should produce a specific gauge reading. Any deviation shows that the gauge or its linkage needs adjustment.

  123. Question 123Air Content of Freshly Mixed Concrete by the Pressure Method

    A second air content test is required on the same concrete. What sample should be used?

    1. The concrete already in the bowl, reworked with a trowel
    2. A fresh, representative sample of the concrete Correct answer.
    3. A sample wetted with water to restore workability
    4. The concrete scraped from the lid back into the bowl

    Explanation

    Concrete that has already been consolidated and pressurized is no longer representative, so a new sample is taken from the batch. Adding water would also change the air content and is never permitted.

  124. Question 124Air Content of Freshly Mixed Concrete by the Pressure Method

    The aggregate correction factor is subtracted from the gauge reading because the aggregates:

    1. hold pores whose air compresses along with the paste air Correct answer.
    2. react with the air-entraining admixture during the test
    3. absorb mix water that would otherwise show on the gauge
    4. raise the density of the concrete and shift the gauge calibration

    Explanation

    Part of the volume change the meter detects comes from air in the voids of the aggregate, not from air in the paste. Subtracting the measured factor removes that contribution so the reported value describes the air in the concrete as a whole.

  125. Question 125Air Content of Freshly Mixed Concrete by the Pressure Method

    Why must the bowl be filled exactly full and struck off level?

    1. So the concrete does not dry out while the lid is clamped
    2. So the lid gasket is not contaminated by cement paste
    3. So the sample weighs the same as a standard batch
    4. So the gauge calibration, based on a known volume, applies Correct answer.

    Explanation

    The gauge graduations assume a fixed volume of concrete in the bowl. If the bowl holds more or less concrete, the same applied pressure produces a different volume change and the reading no longer corresponds to the percent air.

  126. Question 126Air Content of Freshly Mixed Concrete by the Pressure Method

    The gauge reads 4.2% and the aggregate correction factor is 0.8%. The specification requires 5.0% plus or minus 1.0%. What is the reported air content and the correct conclusion?

    1. 3.4%; the concrete meets the specification
    2. 4.2%; the concrete meets the specification
    3. 5.0%; the concrete meets the specification
    4. 3.4%; the concrete does not meet the specification Correct answer.

    Explanation

    The correction factor is subtracted, giving 4.2 minus 0.8, or 3.4% air. The acceptance range is 4.0% to 6.0%, so 3.4% falls below the lower limit and the concrete does not comply.

  127. Question 127Air Content of Freshly Mixed Concrete by the Pressure Method

    When the meter is checked against its calibration vessel, the gauge reads 0.4% instead of the expected value. What does this indicate?

    1. The calibration vessel has absorbed air from the atmosphere
    2. The gauge is fine, since 0.4% is within reading error
    3. The aggregate correction factor should be raised by 0.4%
    4. The meter is out of adjustment and needs servicing Correct answer.

    Explanation

    A rigid calibration vessel contains no compressible air, so any nonzero reading is a direct measure of gauge or linkage error. The meter must be adjusted or repaired, because that same offset would be carried into every test on concrete.

  128. Question 128Air Content of Freshly Mixed Concrete by the Pressure Method

    Why can the pressure meter be used to control air-entraining admixture dosage even though it measures total air?

    1. Because entrapped air is small in well-consolidated concrete Correct answer.
    2. Because the gauge responds only to bubbles below one millimetre
    3. Because the admixture dose is weighed into each batch
    4. Because entrapped air is always a fixed 2 percent of the volume

    Explanation

    In properly consolidated normal-weight concrete, most of the air is the fine entrained bubble system and accidental voids are only a minor fraction. The total air reading therefore tracks the entrained air closely enough for dosage control.

  129. Question 129Air Content of Freshly Mixed Concrete by the Volumetric Method

    The volumetric air meter determines the air content of freshly mixed concrete by measuring which quantity?

    1. The volume of air in a known volume of concrete Correct answer.
    2. The pressure that is required to force water into the concrete
    3. The change in temperature of the concrete during mixing
    4. The mass of water that is displaced by the concrete sample

    Explanation

    The volumetric method measures the total air volume in a known volume of concrete. Water is forced into the concrete under pressure, and the drop in the burette level indicates the air volume. The meter scale is calibrated to read air content directly in percent.

  130. Question 130Air Content of Freshly Mixed Concrete by the Volumetric Method

    Into how many equal layers is the concrete placed in the volumetric air meter container?

    1. Four equal layers
    2. Three equal layers Correct answer.
    3. Two equal layers
    4. Five equal layers

    Explanation

    ASTM C173 requires the container to be filled in three equal layers. Each layer is rodded and tapped before the next layer is added. This ensures uniform consolidation and representative air content.

  131. Question 131Air Content of Freshly Mixed Concrete by the Volumetric Method

    How many times is each layer rodded with the tamping rod in the volumetric air meter test?

    1. 10 times
    2. 15 times
    3. 50 times
    4. 25 times Correct answer.

    Explanation

    Each of the three layers is rodded 25 times with the tamping rod. The strokes are distributed uniformly over the layer. Proper rodding removes large voids that would otherwise be counted as air.

  132. Question 132Air Content of Freshly Mixed Concrete by the Volumetric Method

    After rodding each layer, what is done with the mallet?

    1. The container sides are tapped 10 to 15 times Correct answer.
    2. The burette is struck to release trapped air bubbles
    3. The tamping rod is struck to remove adhering concrete
    4. The lid is struck to help seat the rubber gasket

    Explanation

    Tapping the sides of the container with the mallet after each layer closes voids left by rodding. This helps produce a representative air content. The mallet is not used on the lid, rod, or burette.

  133. Question 133Air Content of Freshly Mixed Concrete by the Volumetric Method

    After the lid is clamped onto the container, water is added through the funnel until what condition is reached?

    1. Water overflows from the pressure relief valve
    2. Water stops flowing into the concrete
    3. Water fills the container to the top of the concrete
    4. Water appears at the top of the burette Correct answer.

    Explanation

    Water is added through the funnel until it appears at the top of the burette, establishing a known initial water level. The top valve is then closed before pressurizing. This initial level is the zero reference for the air reading.

  134. Question 134Air Content of Freshly Mixed Concrete by the Volumetric Method

    How is the air pressure in the volumetric meter brought to the required starting value?

    1. By pumping to the initial pressure mark on the gauge Correct answer.
    2. By opening the top valve and letting the air escape
    3. By tapping the container with the rubber mallet
    4. By filling the burette with water to its top graduation

    Explanation

    A hand pump is used to pressurize the meter until the gauge needle is at the initial pressure mark. This pressure is the value at which the burette scale was calibrated. The gauge is tapped lightly while pumping so the needle does not stick.

  135. Question 135Air Content of Freshly Mixed Concrete by the Volumetric Method

    What does the graduated burette scale on the volumetric air meter indicate after the test?

    1. The slump of the concrete in millimeters
    2. The air content of the concrete in percent Correct answer.
    3. The water-cement ratio of the mixture
    4. The unit weight of the concrete in kilograms per cubic meter

    Explanation

    The burette is graduated so that the drop in water level reads directly as percent air. The meter is calibrated for this purpose using the specified initial pressure. No separate calculation is needed when the meter is properly calibrated.

  136. Question 136Air Content of Freshly Mixed Concrete by the Volumetric Method

    After the final layer is rodded and tapped, how is the concrete surface prepared before the lid is attached?

    1. The surface is mounded above the rim to allow for settlement
    2. The surface is roughened with a trowel to improve the seal
    3. The surface is covered with a thin layer of water
    4. The surface is struck off level with a straightedge Correct answer.

    Explanation

    The concrete is struck off flush with the top of the container using a straightedge. Excess concrete is removed, and the flange is cleaned so the lid gasket seals tightly. A level surface helps ensure the container volume is correct.

  137. Question 137Air Content of Freshly Mixed Concrete by the Volumetric Method

    Which sequence correctly describes the volumetric air meter procedure?

    1. Fill the container, clamp the lid, pressurize, and then rod the concrete
    2. Fill and rod, strike off, clamp lid, fill burette, pressurize, read Correct answer.
    3. Pressurize, fill and rod the container, clamp the lid, and read the burette
    4. Clamp the lid, fill the burette, rod the concrete, and then pressurize the meter

    Explanation

    Concrete is placed and consolidated before the lid is clamped. Water is then added to the burette, the meter is pressurized, and the air content is read from the burette. Rodding after the lid is clamped is not possible.

  138. Question 138Air Content of Freshly Mixed Concrete by the Volumetric Method

    How does the volumetric method account for air trapped in the aggregate?

    1. It applies an aggregate correction factor from a table
    2. It subtracts the aggregate absorption from the reading
    3. It does not use an aggregate correction factor Correct answer.
    4. It measures the aggregate air separately in a second container

    Explanation

    The volumetric method reads total air directly and does not use an aggregate correction factor. Instead, it is limited to concrete made with dense aggregate that does not absorb water. The pressure method is the one that uses an aggregate correction factor.

  139. Question 139Air Content of Freshly Mixed Concrete by the Volumetric Method

    For which concrete is the volumetric air meter method generally unsuitable?

    1. Concrete containing lightweight or highly porous aggregate Correct answer.
    2. Concrete with a slump greater than 100 mm
    3. Concrete with a maximum aggregate size of 25 mm
    4. Concrete made with air-entraining admixtures

    Explanation

    Porous aggregate can absorb the water that is forced into the concrete, causing a false air reading. The method is therefore intended for concrete with dense, non-absorbent aggregate. Air-entrained concrete with normal-weight aggregate is suitable.

  140. Question 140Air Content of Freshly Mixed Concrete by the Volumetric Method

    Why is the pressure gauge tapped lightly while the meter is being pumped?

    1. To prevent the gauge needle from sticking Correct answer.
    2. To increase the pressure more rapidly
    3. To mix the concrete inside the container
    4. To release excess air from the container

    Explanation

    Tapping the gauge helps the needle settle at the true pressure instead of sticking. The operator can then stop pumping at the correct initial pressure mark. This improves the accuracy of the air reading.

  141. Question 141Air Content of Freshly Mixed Concrete by the Volumetric Method

    When should the air content be read from the burette after the valve is opened?

    1. After the water level stops moving Correct answer.
    2. After the meter is shaken for one minute
    3. After the gauge reaches zero pressure
    4. Immediately when the valve is opened

    Explanation

    The water level drops as water is forced into the concrete and then stabilizes. The reading is taken at the stable level. Reading too early can give an incorrect air content.

  142. Question 142Air Content of Freshly Mixed Concrete by the Volumetric Method

    What effect does insufficient rodding have on the volumetric air content result?

    1. It raises the reading by leaving entrapped voids Correct answer.
    2. It lowers the reading by compressing the concrete
    3. It has no effect because the meter measures only entrained air
    4. It makes the result depend only on the aggregate size

    Explanation

    Insufficient rodding leaves large entrapped air pockets in the concrete. The meter measures total air, so these voids are counted and the reading is too high. Proper rodding of each layer is needed for a representative result.

  143. Question 143Air Content of Freshly Mixed Concrete by the Volumetric Method

    Why must the flange of the container and the lid gasket be cleaned before the lid is clamped?

    1. To prevent concrete from sticking to the burette
    2. To make the lid easier to lift
    3. To ensure a tight pressure seal Correct answer.
    4. To change the volume of the container

    Explanation

    Concrete or grit on the flange can prevent the gasket from sealing. A leaking lid causes pressure loss and an inaccurate air reading. Cleaning the flange and gasket is therefore part of the procedure.

  144. Question 144Air Content of Freshly Mixed Concrete by the Volumetric Method

    Why is the top valve of the burette closed before the meter is pressurized?

    1. To let the gauge read the water pressure
    2. To keep the water from freezing in the tube
    3. To seal the water column for the reading Correct answer.
    4. To allow air to escape from the burette

    Explanation

    Closing the top valve seals the burette so that the water level can respond to pressure changes in the container. If the valve were open, water could be forced out and the reading would be lost. The valve is opened only when the meter is being filled or vented.

  145. Question 145Air Content of Freshly Mixed Concrete by the Volumetric Method

    Which type of air does the volumetric meter measure in fresh concrete?

    1. Only air dissolved in the mixing water
    2. Only entrained air
    3. Both entrained and entrapped air Correct answer.
    4. Only entrapped air

    Explanation

    The volumetric method measures the total air volume in the concrete, which includes both intentionally entrained air and accidentally entrapped air. It does not separate the two types. Other tests or petrographic examination may be needed to distinguish them.

  146. Question 146Air Content of Freshly Mixed Concrete by the Volumetric Method

    Why is the exact volume of the air meter container important?

    1. It sets the pressure at which the gauge is read
    2. The burette scale is calibrated to that volume Correct answer.
    3. It controls the number of rodding strokes required
    4. It determines the amount of water used to fill the burette

    Explanation

    The burette scale reads percent air only if the container volume is the calibrated value. If the container is damaged or the volume is wrong, the same water-level drop corresponds to a different percentage. The container volume must therefore be maintained and checked.

  147. Question 147Air Content of Freshly Mixed Concrete by the Volumetric Method

    Why does the burette scale read air content directly in percent when the meter is at the specified pressure?

    1. The pressure gauge converts its reading directly into a percentage
    2. The concrete expands when pressure is applied and pushes water upward
    3. The scale is calibrated for water displaced by compressed air Correct answer.
    4. The water dissolves the air and the scale measures the dissolved volume

    Explanation

    When pressure is applied, water is forced into the concrete and compresses the air in the voids. The water level in the burette drops by an amount related to the original air volume. The scale is calibrated so that this drop reads as percent air at the specified pressure.

  148. Question 148Air Content of Freshly Mixed Concrete by the Volumetric Method

    What distinguishes the volumetric method from the pressure method for air content?

    1. It reads the change in water level directly Correct answer.
    2. The pressure method measures air by water displacement
    3. The volumetric method requires an aggregate correction factor
    4. The volumetric method is based on Boyle's law

    Explanation

    The volumetric method measures the drop in the burette water level to determine air content directly. The pressure method measures a pressure change and applies Boyle's law. The volumetric method does not use an aggregate correction factor, while the pressure method does.

  149. Question 149Air Content of Freshly Mixed Concrete by the Volumetric Method

    What error occurs if the volumetric method is used on concrete made with highly porous aggregate?

    1. The air content is reported too low
    2. The air content is reported as zero
    3. The air content is reported too high Correct answer.
    4. The air content is unaffected but the slump changes

    Explanation

    Water forced into the concrete can enter pores in the aggregate as well as air voids. The extra water displacement is interpreted as air, so the reading is falsely high. This is why the method is not suitable for porous aggregate.

  150. Question 150Air Content of Freshly Mixed Concrete by the Volumetric Method

    If the meter is pressurized below the specified initial pressure, how is the air content reading affected?

    1. It is corrected automatically by the water level
    2. It is reported lower than the true value Correct answer.
    3. It is reported higher than the true value
    4. It is unaffected because the scale is linear

    Explanation

    Lower pressure forces less water into the concrete, so the burette water level drops less. Since the scale is calibrated for the specified pressure, the indicated air content is lower than the true value. The gauge must be at the initial pressure mark.

  151. Question 151Air Content of Freshly Mixed Concrete by the Volumetric Method

    What should be done with the pressure before the lid is removed after the test?

    1. It should be transferred to the burette
    2. It should be released through the valve Correct answer.
    3. It should be increased to keep the lid tight
    4. It should be left as it is to protect the concrete

    Explanation

    The pressure must be released before the lid is unclamped. Removing the lid under pressure can be dangerous and can disturb the meter. The valves are used to vent the pressure safely.

  152. Question 152Air Content of Freshly Mixed Concrete by the Volumetric Method

    What maintenance practice helps keep the volumetric air meter accurate?

    1. Cleaning and drying the meter after each use Correct answer.
    2. Leaving concrete residue on the gasket to improve sealing
    3. Coating the burette with oil after each test
    4. Storing the meter filled with water

    Explanation

    Dried concrete and sediment can clog valves and change the container volume. The meter should be cleaned and dried after each use, and the gasket should be kept clean. Regular maintenance helps preserve the calibration.

  153. Question 153Making and Curing Concrete Test Specimens in the Field

    In accordance with ASTM C172, at what point during discharge should a sample of concrete be obtained for field specimens?

    1. From the stationary mixer drum before any concrete is discharged into the transporter
    2. The last portion discharged from the mixer
    3. The first portion discharged from the mixer
    4. Middle portion of the batch, between 15 % and 85 % of discharge Correct answer.

    Explanation

    A representative sample is taken after all mixing, from the middle portion of the discharge between 15 % and 85 %. The first and last portions may be segregated or otherwise unrepresentative of the whole batch. Compositing portions over the middle discharge interval also helps represent the batch.

  154. Question 154Making and Curing Concrete Test Specimens in the Field

    What is the minimum volume of concrete sample required for making strength specimens in the field?

    1. 3 ft³ (85 L)
    2. 0.25 ft³ (7 L)
    3. 1 ft³ (28 L) Correct answer.
    4. 6 ft³ (170 L)

    Explanation

    ASTM C31 requires a field sample of at least 1 ft³ (28 L) so that sufficient specimens and tests can be made. A smaller sample may not provide enough concrete or may not represent the batch. Larger samples are acceptable when extra tests are needed.

  155. Question 155Making and Curing Concrete Test Specimens in the Field

    When molding a 6 by 12 in. (150 by 300 mm) cylindrical specimen, how many layers of concrete are placed?

    1. Four layers
    2. Three layers Correct answer.
    3. Two layers
    4. One layer

    Explanation

    A 6 by 12 in. cylinder is filled in three approximately equal layers, and each layer is rodded 25 times. A 4 by 8 in. mold uses two layers. The layer depth in a 6 by 12 in. mold is about 4 in.

  156. Question 156Making and Curing Concrete Test Specimens in the Field

    How many strokes of the tamping rod are required for each layer when molding standard cylindrical specimens?

    1. 15 strokes
    2. 25 strokes Correct answer.
    3. 10 strokes
    4. 20 strokes

    Explanation

    Each layer in a standard cylinder is rodded 25 times uniformly over its cross section. The same stroke count applies to both 4 by 8 in. and 6 by 12 in. cylinders. The rod is distributed so that the entire layer is consolidated.

  157. Question 157Making and Curing Concrete Test Specimens in the Field

    After rodding each layer of a cylinder, what is the required tapping procedure?

    1. Tap the mold only 1 to 2 times with a heavy hammer
    2. Vibrate the mold for approximately 5 seconds on a vibrating table
    3. Strike the mold sharply once on each of the four sides
    4. Tap the mold 10 to 15 times with a mallet Correct answer.

    Explanation

    Tapping the outside of the mold 10 to 15 times with a mallet after each layer closes voids left by rodding. This helps produce a dense, uniform specimen. Tapping should not be so severe that it damages the mold or causes segregation.

  158. Question 158Making and Curing Concrete Test Specimens in the Field

    During the initial curing period, field specimens must be stored within what temperature range?

    1. 60 to 80 °F (16 to 27 °C) Correct answer.
    2. 40 to 60 °F (4 to 16 °C)
    3. 80 to 100 °F (27 to 38 °C)
    4. 70 to 90 °F (21 to 32 °C)

    Explanation

    ASTM C31 requires the initial curing environment to be maintained at 60 to 80 °F (16 to 27 °C). Temperatures outside this range can alter strength development and make results unrepresentative. Specimens must also be kept moist and protected from freezing.

  159. Question 159Making and Curing Concrete Test Specimens in the Field

    How should field specimens be identified before they are transported to the laboratory?

    1. By durable marking on the mold or specimen Correct answer.
    2. By relying on the laboratory to assign a number later
    3. By placing a loose paper tag inside the mold
    4. By writing on the concrete with water-soluble chalk

    Explanation

    Specimens must be identified by a durable mark on the mold or on the specimen itself so they can be traced to the sample location and batch. Identification should be applied before the specimen leaves the field. Loose tags can be lost and are not a reliable means.

  160. Question 160Making and Curing Concrete Test Specimens in the Field

    Which tamping rod diameter is specified for molding 4 by 8 in. (100 by 200 mm) cylindrical specimens?

    1. 1/2 in. (13 mm)
    2. 3/8 in. (10 mm) Correct answer.
    3. 1/4 in. (6 mm)
    4. 5/8 in. (16 mm)

    Explanation

    A 3/8 in. (10 mm) diameter rod is used for 4 by 8 in. cylinders, while a 5/8 in. (16 mm) rod is used for 6 by 12 in. cylinders. The smaller rod fits the smaller mold and provides proper consolidation. The rod must have a rounded tip.

  161. Question 161Making and Curing Concrete Test Specimens in the Field

    When rodding the second or third layer of a cylinder, the rod should penetrate into the underlying layer by approximately how much?

    1. 1 in. (25 mm) Correct answer.
    2. 2 in. (50 mm)
    3. The full depth of the underlying layer
    4. 1/4 in. (6 mm)

    Explanation

    The rod should penetrate about 1 in. (25 mm) into the layer below so that the layers are bonded together. Penetrating too deeply can disturb the lower layer, while not penetrating can leave a plane of weakness. The bottom layer is rodded throughout its depth.

  162. Question 162Making and Curing Concrete Test Specimens in the Field

    What is the proper procedure for finishing the top surface of a molded cylinder?

    1. Leave the surface rounded above the mold rim
    2. Strike off flat with a straightedge or trowel Correct answer.
    3. Trowel the surface to a smooth, polished finish
    4. Add a small amount of mortar to fill any low spots on the surface

    Explanation

    After the final layer is consolidated, the surface is struck off even with the top of the mold using a straightedge or trowel. The surface should be flat and should not be retempered with mortar. Excess troweling can produce a nonrepresentative surface.

  163. Question 163Making and Curing Concrete Test Specimens in the Field

    What is the maximum duration of the initial curing period for field specimens before they are moved to standard curing?

    1. 24 h
    2. 72 h
    3. 7 days
    4. 48 h Correct answer.

    Explanation

    The initial curing period on site shall not exceed 48 h. During this time the specimens must be kept at 60 to 80 °F and protected from moisture loss and freezing. After initial curing, they are moved to standard moist curing.

  164. Question 164Making and Curing Concrete Test Specimens in the Field

    What are the required conditions for standard curing of test specimens after initial curing?

    1. 60 ± 5 °F (16 ± 3 °C) and 50 % relative humidity
    2. Any temperature as long as the specimens remain wet
    3. 73.4 ± 3 °F (23 ± 2 °C) and 100 % relative humidity Correct answer.
    4. 80 ± 5 °F (27 ± 3 °C) and 75 % relative humidity

    Explanation

    Standard curing requires a moist environment at 73.4 ± 3 °F (23 ± 2 °C), either in a moist room at 100 % relative humidity or in lime-saturated water. These conditions provide a consistent basis for comparing strength results. Field curing is different and serves other purposes.

  165. Question 165Making and Curing Concrete Test Specimens in the Field

    At what time after molding should cylindrical specimens normally be removed from their molds?

    1. 72 ± 12 h
    2. 8 ± 2 h
    3. 24 ± 8 h Correct answer.
    4. 16 ± 4 h

    Explanation

    Specimens are normally demolded at 24 ± 8 h after molding, once they have sufficient strength to be handled without damage. Demolding too early can damage the specimen, while leaving it too long can interfere with curing. The exact time may depend on strength development.

  166. Question 166Making and Curing Concrete Test Specimens in the Field

    What is the primary purpose of making field-cured specimens alongside standard-cured specimens?

    1. To replace standard-cured specimens for acceptance testing
    2. To estimate the cement content of the concrete mixture
    3. To evaluate curing and protection of concrete in the structure Correct answer.
    4. To check the calibration of the compression testing machine before use

    Explanation

    Field-cured specimens are stored as close as practicable to the structure and are used to evaluate whether the in-place concrete has been properly cured and protected. Standard-cured specimens are the basis for acceptance. Field-cured specimens are not a substitute for standard curing.

  167. Question 167Making and Curing Concrete Test Specimens in the Field

    How should a reusable cylinder mold be prepared before concrete is placed?

    1. Coat the inside with a thick layer of grease
    2. Apply a thin film of release agent Correct answer.
    3. Line the inside with absorbent paper
    4. Leave the inside dry and uncoated

    Explanation

    A thin film of mineral oil or other suitable release agent prevents the concrete from bonding to the mold. Excess release agent can collect and affect the concrete surface. Molds must also be clean, leakproof, and nonabsorbent.

  168. Question 168Making and Curing Concrete Test Specimens in the Field

    How should field specimens be protected during initial curing to prevent moisture loss?

    1. Cover them with plastic sheeting or wet burlap Correct answer.
    2. Submerge them immediately in water before they have set
    3. Place them in an open, dry area with good ventilation
    4. Store them uncovered in direct sunlight for the entire period

    Explanation

    During initial curing, specimens must be protected from evaporation by covering with plastic or wet burlap and keeping them moist. Direct sunlight and dry air can cause plastic shrinkage and cracking. They should not be submerged before they have set.

  169. Question 169Making and Curing Concrete Test Specimens in the Field

    When obtaining a composite sample from a truck mixer, how should the portions be taken?

    1. All at once from the first part of the discharge
    2. Only from the last part of the discharge
    3. At regular intervals during middle discharge Correct answer.
    4. From the mixer drum before discharging

    Explanation

    A composite sample is obtained by taking portions at several regular intervals during discharge, generally between 15 % and 85 % of the batch. This reduces the effect of segregation and variation within the batch. Combining the portions gives a representative sample.

  170. Question 170Making and Curing Concrete Test Specimens in the Field

    How should field specimens be stored during the initial curing period?

    1. Stacked on top of each other immediately
    2. On the ground near the mixer
    3. On a soft cushion to absorb shock and vibration
    4. On a rigid, level, vibration-free support Correct answer.

    Explanation

    Specimens must be stored on a rigid, level support that is free from vibration and protected from sunlight and evaporation. Movement or vibration before the concrete has set can damage the specimen. Stacking freshly molded specimens can also cause distortion.

  171. Question 171Making and Curing Concrete Test Specimens in the Field

    For concrete with a nominal maximum coarse aggregate size of 1 in. (25 mm), which cylinder mold size is permitted?

    1. 4 by 8 in. (100 by 200 mm) Correct answer.
    2. No standard cylinder mold is permitted
    3. 3 by 6 in. (75 by 150 mm)
    4. 2 by 4 in. (50 by 100 mm)

    Explanation

    ASTM C31 permits 4 by 8 in. molds for concrete with nominal maximum aggregate size not exceeding 1 in. (25 mm). The specimen diameter must be at least three times the nominal maximum aggregate size. Smaller molds would not satisfy that requirement.

  172. Question 172Making and Curing Concrete Test Specimens in the Field

    A set of field specimens is initially cured at 95 °F (35 °C) for 24 h instead of the specified range. What is the most likely effect on the measured compressive strength?

    1. The strength will be unaffected because curing temperature does not matter after molding
    2. The strength will be consistently lower at all ages and cannot be corrected
    3. Early strength may increase but later strength may decrease Correct answer.
    4. The strength will be exactly the same as standard-cured specimens

    Explanation

    Initial curing above the specified 60 to 80 °F range accelerates early hydration, which can increase early strength but may reduce later strength development. Because the specimens are not representative of standard curing, the results may not be valid for acceptance. Temperature during initial curing is therefore controlled.

  173. Question 173Making and Curing Concrete Test Specimens in the Field

    A project requires both standard-cured and field-cured cylinders. Which statement correctly describes their use?

    1. Only field-cured cylinders are required when the structure will be opened early
    2. Both sets are averaged together for acceptance
    3. Standard-cured cylinders are used for acceptance, and field-cured cylinders are used for in-place curing evaluation Correct answer.
    4. Field-cured cylinders are used for acceptance, and standard-cured cylinders are used for curing evaluation

    Explanation

    Standard-cured specimens are cured under controlled conditions and are used for acceptance and quality control. Field-cured specimens are stored near the structure and are used to determine whether the concrete in place has been adequately cured or protected. The two sets serve different purposes and are not averaged together for acceptance.

  174. Question 174Making and Curing Concrete Test Specimens in the Field

    A technician takes a strength sample from the first 10 % of the discharge because the truck is running late. Why is this sample unacceptable?

    1. The sample volume will be too small
    2. The concrete has not yet begun to hydrate
    3. First portion may not represent the batch Correct answer.
    4. The first portion is always too cold to test

    Explanation

    Sampling is required from the middle portion of the batch, between 15 % and 85 % of discharge, because the first portion can be segregated or otherwise unrepresentative. Using it can bias the strength results. The problem is representativeness, not temperature, volume, or hydration.

  175. Question 175Making and Curing Concrete Test Specimens in the Field

    A 6 by 12 in. cylinder is rodded only 15 times per layer. What is the most likely result?

    1. Voids may form and strength may decrease Correct answer.
    2. The specimen will be unaffected because 15 strokes are sufficient
    3. The mold will leak because the concrete is not compacted
    4. The specimen will have a higher strength because less disturbance occurs

    Explanation

    Underc consolidation leaves entrapped air voids and can reduce the density and measured compressive strength of the specimen. The specified 25 strokes per layer are needed for proper consolidation. The result would not be a valid representation of the concrete.

  176. Question 176Making and Curing Concrete Test Specimens in the Field

    Field specimens remain in initial curing for 72 h before being moved to the moist room. What is the main concern?

    1. The molds will absorb water and shrink
    2. The concrete will carbonate and lose all strength
    3. Results may not be comparable to standard curing Correct answer.
    4. The specimens will gain too much strength to test

    Explanation

    The initial curing period is limited to 48 h so that specimens are moved to standard curing in a timely manner. Extending initial curing beyond that period changes the curing history and can affect the strength results. The concern is comparability and validity, not mold absorption or total loss of strength.

  177. Question 177Capping and Compressive Strength Testing of Cylindrical Specimens

    At what rate shall a compressive load be applied to a standard concrete cylinder during a compression test?

    1. 35 ± 7 psi/s Correct answer.
    2. 50 ± 10 psi/s
    3. 20 ± 5 psi/s
    4. 70 ± 14 psi/s

    Explanation

    The standard loading rate for compressive strength testing of cylindrical specimens is 35 ± 7 psi/s, which is equivalent to 0.25 ± 0.05 MPa/s. This rate is applied continuously without shock until the specimen fails. Rates outside this range can bias the measured strength.

  178. Question 178Capping and Compressive Strength Testing of Cylindrical Specimens

    What is the minimum number of cylindrical specimens normally required to determine the compressive strength of a concrete test batch?

    1. Three Correct answer.
    2. Six
    3. Two
    4. One

    Explanation

    A compressive strength test normally consists of at least three cylindrical specimens tested at the specified age. The results are averaged to represent the batch. Testing only one or two specimens does not provide the required reliability.

  179. Question 179Capping and Compressive Strength Testing of Cylindrical Specimens

    How closely must the capped end of a cylinder approach a true plane?

    1. Within 0.02 in.
    2. Within 0.005 in.
    3. Within 0.01 in.
    4. Within 0.002 in. Correct answer.

    Explanation

    The cap surface must be plane within 0.002 in. (0.05 mm). This tolerance ensures that load is distributed uniformly across the specimen end. A cap outside this tolerance can cause eccentric loading and an invalid strength result.

  180. Question 180Capping and Compressive Strength Testing of Cylindrical Specimens

    Which material is commonly used to cap hard, surface-dry concrete cylinders before compression testing?

    1. Clean sand
    2. Sulfur mortar Correct answer.
    3. Portland cement paste
    4. Clay

    Explanation

    Sulfur mortar is a standard capping material because it hardens quickly and can be finished to a plane surface within the required tolerance. It bonds adequately to a dry, clean cylinder end. Other materials listed do not provide the needed strength and planeness.

  181. Question 181Capping and Compressive Strength Testing of Cylindrical Specimens

    At what age is the specified compressive strength of concrete normally determined for acceptance?

    1. 28 days Correct answer.
    2. 7 days
    3. 56 days
    4. 14 days

    Explanation

    The specified compressive strength is normally based on tests of specimens at 28 days. Earlier-age tests, such as 7-day tests, are used for informational or quality-control purposes. Later ages may be specified for special projects but are not the standard acceptance age.

  182. Question 182Capping and Compressive Strength Testing of Cylindrical Specimens

    If the ends of a cylinder are not plane within the required tolerance, what must be done before compression testing?

    1. Test the specimen without preparation
    2. Discard the specimen
    3. Increase the loading rate
    4. Cap or grind the ends Correct answer.

    Explanation

    Cylinder ends that do not meet the planeness tolerance must be capped or ground so that load is applied uniformly. Testing an unprepared end can cause stress concentrations and premature failure. Discarding the specimen is unnecessary when proper end preparation is possible.

  183. Question 183Capping and Compressive Strength Testing of Cylindrical Specimens

    Sulfur mortar used for capping should be maintained within which temperature range during use?

    1. 265 to 290°F Correct answer.
    2. 300 to 330°F
    3. 200 to 220°F
    4. 350 to 400°F

    Explanation

    Sulfur mortar is kept at approximately 265 to 290°F (130 to 143°C) so that it remains fluid enough to form a thin cap without overheating. Excessive temperature can degrade the material, while too low a temperature makes it too viscous. Proper temperature control helps produce a sound, plane cap.

  184. Question 184Capping and Compressive Strength Testing of Cylindrical Specimens

    After a sulfur mortar cap is formed, what is the minimum time it should be allowed to harden before the specimen is tested?

    1. 4 hours
    2. 30 minutes
    3. 2 hours Correct answer.
    4. 1 hour

    Explanation

    Sulfur mortar caps should be allowed to harden for at least 2 hours before testing. This waiting period allows the cap to develop sufficient strength to transmit the test load. Testing too soon can crush or deform the cap.

  185. Question 185Capping and Compressive Strength Testing of Cylindrical Specimens

    A 6-in. diameter cylinder has a cross-sectional area of about 28.3 in². At the standard loading rate of 35 psi/s, what load rate should be applied?

    1. About 250 lbf/s
    2. About 2,000 lbf/s
    3. About 990 lbf/s Correct answer.
    4. About 500 lbf/s

    Explanation

    Load rate equals stress rate multiplied by cross-sectional area: 35 psi/s × 28.3 in² ≈ 990 lbf/s. This corresponds to the standard stress rate for a 6-in. cylinder. Applying the load at this rate keeps the test within the specified tolerance.

  186. Question 186Capping and Compressive Strength Testing of Cylindrical Specimens

    How often must a compression testing machine be verified for accuracy?

    1. Annually Correct answer.
    2. Every five years
    3. Weekly
    4. Monthly

    Explanation

    Compression testing machines must be verified at least annually to confirm that indicated loads are accurate within the required tolerance. Verification is also required after certain repairs or modifications. Regular verification protects the validity of strength results.

  187. Question 187Capping and Compressive Strength Testing of Cylindrical Specimens

    To what precision should the diameter of a test cylinder be measured for calculating cross-sectional area?

    1. Nearest 0.5 in.
    2. Nearest 0.01 in. Correct answer.
    3. Nearest 0.1 in.
    4. Nearest 0.001 in.

    Explanation

    The cylinder diameter is measured to the nearest 0.01 in. (0.25 mm) so that the cross-sectional area is accurate. Diameter is usually determined from two measurements taken at right angles near mid-height. This precision supports a reliable strength calculation.

  188. Question 188Capping and Compressive Strength Testing of Cylindrical Specimens

    What characteristic is required of the plate used to form a sulfur mortar cap?

    1. It should be flexible.
    2. It should be porous.
    3. It should be flat and rigid. Correct answer.
    4. It should be made of wood.

    Explanation

    The capping plate must be flat and rigid so that the cap is formed to the required planeness. A plate that flexes or wears can produce a cap that is not perpendicular to the cylinder axis. The plate should also be clean and lightly coated with a suitable release agent.

  189. Question 189Capping and Compressive Strength Testing of Cylindrical Specimens

    At what point in specimen preparation are sulfur mortar caps normally applied?

    1. While the concrete is still being molded
    2. After the specimen has been tested
    3. Before the specimen is cured
    4. After curing, when the specimen surface is dry Correct answer.

    Explanation

    Caps are applied after the curing period, when the cylinder ends are clean and surface dry. A dry surface allows the sulfur mortar to bond properly. Capping before curing or during molding would interfere with proper specimen preparation.

  190. Question 190Capping and Compressive Strength Testing of Cylindrical Specimens

    What is the maximum permitted thickness of a sulfur mortar cap?

    1. 1/2 in.
    2. 3/16 in.
    3. 1/8 in. Correct answer.
    4. 1/4 in.

    Explanation

    A sulfur mortar cap should not exceed 1/8 in. (3 mm) in thickness. A thicker cap can deform or fail under load and may not accurately transmit stress to the concrete. The cap should be as thin as practical while still providing a plane surface.

  191. Question 191Capping and Compressive Strength Testing of Cylindrical Specimens

    Unbonded neoprene caps are generally permitted for use on concrete cylinders with compressive strengths up to approximately what value?

    1. 10,000 psi
    2. 7,000 psi Correct answer.
    3. 4,000 psi
    4. 12,000 psi

    Explanation

    Unbonded neoprene caps are generally limited to concrete with compressive strengths up to about 7,000 psi. At higher strengths, the pads may not distribute load reliably and bonded caps or grinding are required. The exact limit should always be confirmed from the governing test method.

  192. Question 192Capping and Compressive Strength Testing of Cylindrical Specimens

    A completed cap is found to be outside the permitted planeness tolerance. What is the appropriate action?

    1. Reduce the loading rate
    2. Remove the cap and replace it Correct answer.
    3. Test the specimen as it is
    4. Increase the loading rate

    Explanation

    A cap that is not within the planeness tolerance must be removed and replaced, or the end must be ground, before testing. Testing an out-of-plane cap can cause eccentric loading and an invalid result. Adjusting the loading rate does not correct the geometry.

  193. Question 193Capping and Compressive Strength Testing of Cylindrical Specimens

    Which statement best describes the bearing blocks of a compression testing machine?

    1. They should be made of wood
    2. They should be smaller than the specimen diameter
    3. They should be softer than the specimen
    4. They should be harder than the specimen and have plane bearing faces Correct answer.

    Explanation

    Bearing blocks must be hard enough to resist deformation and must have plane faces so that load is applied uniformly. The upper block is typically fitted with a spherical seat to accommodate slight specimen misalignment. Soft or undersized blocks can cause inaccurate results.

  194. Question 194Capping and Compressive Strength Testing of Cylindrical Specimens

    Cylinders awaiting a 28-day test should be stored in water maintained at what temperature?

    1. 65 ± 2°F
    2. 60 ± 5°F
    3. 73.5 ± 3.5°F Correct answer.
    4. 80 ± 5°F

    Explanation

    Standard moist curing requires water at 73.5 ± 3.5°F (23 ± 2°C). This temperature range supports normal strength development and consistent test results. Storage outside this range can affect the measured strength.

  195. Question 195Capping and Compressive Strength Testing of Cylindrical Specimens

    A 4-in. diameter cylinder has a cross-sectional area of about 8,107 mm². At a stress rate of 0.25 MPa/s, what load rate is required?

    1. About 2.0 kN/s Correct answer.
    2. About 8.0 kN/s
    3. About 4.5 kN/s
    4. About 1.0 kN/s

    Explanation

    Load rate equals stress rate multiplied by area: 0.25 N/mm²/s × 8,107 mm² ≈ 2,027 N/s, or about 2.0 kN/s. This is the metric equivalent of the standard loading rate for a 4-in. cylinder. The same calculation approach applies to other diameters.

  196. Question 196Capping and Compressive Strength Testing of Cylindrical Specimens

    Compressive strength is calculated by dividing the maximum load by which quantity?

    1. Specimen length
    2. Specimen volume
    3. Specimen circumference
    4. Cross-sectional area Correct answer.

    Explanation

    Compressive strength equals maximum load divided by the cross-sectional area of the cylinder. Area is computed from the measured diameter. Length, volume, and circumference are not used in the strength calculation.

  197. Question 197Capping and Compressive Strength Testing of Cylindrical Specimens

    Before testing a cylinder capped with sulfur mortar, what should be confirmed?

    1. The cap has been heated just before testing
    2. The specimen has been soaked for 24 hours after capping
    3. The cap has been removed
    4. The caps are hard and within the planeness tolerance Correct answer.

    Explanation

    The cap must be hard and plane before the specimen is tested. The cap should also be sound and free of voids or cracks. Testing a soft or uneven cap can produce a premature or invalid failure.

  198. Question 198Capping and Compressive Strength Testing of Cylindrical Specimens

    A 6-in. cylinder has an average measured diameter of 5.98 in. What cross-sectional area should be used to calculate its compressive strength?

    1. 27.0 in²
    2. 28.1 in² Correct answer.
    3. 28.3 in²
    4. 36.0 in²

    Explanation

    Area equals π times diameter squared divided by 4: π × (5.98)² / 4 ≈ 28.1 in². The measured diameter, not the nominal 6-in. diameter, should be used. Using the nominal diameter would slightly overstate the area and understate the strength.

  199. Question 199Capping and Compressive Strength Testing of Cylindrical Specimens

    What is the primary purpose of capping a concrete cylinder before compression testing?

    1. To shorten the required curing period
    2. To provide a smooth, plane surface for uniform load application Correct answer.
    3. To increase the concrete strength
    4. To increase the specimen height

    Explanation

    Capping provides a smooth, plane bearing surface so that the compression machine applies load uniformly across the specimen end. Uniform loading is necessary for a valid strength result. Capping does not change the concrete's strength or curing requirements.

  200. Question 200Capping and Compressive Strength Testing of Cylindrical Specimens

    Which feature on the upper bearing block of a compression machine helps accommodate slight misalignment of a cylinder?

    1. A rubber pad
    2. A wooden insert
    3. A spherical seat Correct answer.
    4. A fixed flat plate with no seat

    Explanation

    The upper bearing block normally has a spherical seat that allows slight rotation so the bearing face can align with the specimen end. This helps distribute load evenly. A rigid, unseated block can produce eccentric loading if the specimen is slightly out of alignment.

ACI Field Testing I flashcards

32 cards. Read the term and the definition here. The deck at the top of this page is optional.

ASTM C172
Standard practice for sampling freshly mixed concrete; requires a representative sample from the middle portion of the batch, protected from contamination and evaporation.
Representative sample
A sample that contains the same proportions of ingredients as the batch; obtained from the middle discharge and not from segregated or contaminated material.
Composite sample
A sample made by combining increments from several portions of a batch; it is remixed before testing so the result represents the whole batch.
Sampling receptacle
A clean, dampened container used to catch fresh concrete; it must not contain set concrete, dirt, or chemicals that could alter the sample.
ASTM C1064
Standard test method for temperature of freshly mixed concrete; uses a calibrated immersion thermometer and requires reading after stabilization.
Thermometer immersion depth
At least 3 in. (75 mm) of the thermometer sensing portion must be immersed in concrete, away from the container walls.
Temperature report precision
Report fresh concrete temperature to the nearest 0.5°C (1°F), matching the precision of the calibrated thermometer and specification.
Infrared thermometer limitation
An infrared device measures surface temperature and is not an acceptable substitute for the ASTM C1064 immersion measurement of fresh concrete.
ASTM C143
Standard slump test for hydraulic cement concrete; uses a 12-in. mold, three layers, and 25 rod strokes per layer.
Slump mold dimensions
The standard slump cone is 12 in. (300 mm) high, with an 8 in. (200 mm) bottom diameter and a 4 in. (100 mm) top diameter.
Slump measurement
The vertical drop from the original top of the mold to the displaced center of the concrete, reported to the nearest 1/4 in. (5 mm).
Slump test timing
The entire slump test must be completed within 2.5 min after sampling; a sample that has stood is not retested.
ASTM C138
Standard test method for density, yield, and gravimetric air content of concrete using a calibrated measure of known volume.
Unit weight formula
Density equals the mass of concrete in the measure divided by the measure volume; report as lb/ft³ or kg/m³.
Yield formula
Yield equals total batch mass divided by measured unit weight; relative yield compares actual yield with design volume.
Gravimetric air formula
Air content equals 100 times one minus measured unit weight divided by theoretical air-free unit weight.
ASTM C231
Standard pressure-method test for air content of fresh concrete; based on Boyle's law and requires an aggregate correction factor.
Aggregate correction factor
A value subtracted from the pressure meter gauge reading to account for air trapped in porous aggregate; determined for the specific aggregate combination.
Pressure meter leakage
Leakage at the lid or valve causes the gauge to read incorrectly; clean the flange and seal the meter before pressurizing.
Pressure method limitation
The pressure method may be unreliable for highly porous or lightweight aggregate unless the aggregate correction is verified.
ASTM C173
Standard volumetric method for air content; removes air from a concrete sample by agitation and reads the water-level drop.
Volumetric air reading
Air content is read directly from the graduated neck of the meter after repeated agitation until the reading stabilizes.
Volumetric meter agitation
Invert and roll the meter repeatedly to release entrapped air; continue until the air volume reading no longer changes.
Volumetric method suitability
Best suited to dense-aggregate concrete that can be agitated; stiff mixtures or gas-releasing aggregate can give inaccurate results.
ASTM C31
Standard practice for making and curing concrete test specimens in the field; covers molds, consolidation, initial curing, and transport.
6 x 12 in. cylinder layers
Fill a 6 x 12 in. cylinder in three equal layers, rodding each layer 25 times with the standard rod.
4 x 8 in. cylinder layers
Fill a 4 x 8 in. cylinder in two equal layers, rodding each layer 25 times with the standard rod.
Initial curing temperature
Keep freshly made field specimens at 60 to 80°F (16 to 27°C) and prevent moisture loss for 24 ± 8 h before demolding.
ASTM C617
Standard practice for capping cylindrical concrete specimens; caps must be flat, perpendicular to the axis, and sound.
Compressive strength formula
Compressive strength equals the maximum test load divided by the cylinder cross-sectional area, reported in psi or MPa.
ASTM C39
Standard test method for compressive strength of cylindrical specimens; specifies centering, loading rate, and reporting.
Capping defect effect
An uneven, thick, or voided cap can create eccentric loading and lower the measured compressive strength.

ACI Field Testing I study guide

Sampling Freshly Mixed Concrete

Why sampling matters

Sampling is the first point at which a test result can be invalidated. The sample must represent the entire batch, not the easiest concrete to reach. Take a composite sample from the middle portion of the discharge, using at least three increments taken across the discharge. Do not take the first or last material from a truck or chute. The minimum sample size is about 1 ft³ (28 L); for strength cylinders plus slump, air, and temperature tests, 1.5 ft³ is safer. Obtain the sample within 15 minutes of discharge and begin tests promptly.

Handling and remixing

Collect the sample in a clean, damp container and protect it from evaporation, rain, and contamination. Before testing, remix the sample with a scoop or shovel so that it is uniform; do not use a trowel to stir only the surface. Complete slump, air, and temperature tests within 15 minutes of sampling. If the concrete has begun to stiffen, do not add water to make it workable.

Traps and rule of thumb

Common traps include sampling only from the top of a wheelbarrow, taking a single scoop, sampling from the very beginning of discharge, and letting the sample sit while paperwork is completed. Another trap is testing a sample that has been remixed with water or that has dried at the edges.

Rule of thumb: one 6 in. by 12 in. cylinder contains about 0.196 ft³ of concrete, so three cylinders require about 0.59 ft³. With slump, air, and temperature, allow at least 1 ft³ and preferably 1.5 ft³. If the sample is short, discard it and resample; do not stretch it.

Temperature of Freshly Mixed Concrete

Thermometer and placement

Temperature is a simple test with strict details. Use a thermometer with accuracy of at least ±1°F (±0.5°C) and a range that covers the expected concrete temperature. The concrete sample must be at least 3 in. (75 mm) deep, and the thermometer must be immersed at least 3 in. (75 mm) into the concrete and kept at least 3 in. from the container walls. Leave it in place for at least 2 minutes, then read it while the thermometer is still in the concrete. Record to the nearest 1°F (0.5°C).

Sample conditions

Measure temperature on a representative sample within 15 minutes of sampling. Protect the sample from direct sunlight, wind, and hot or cold surfaces; these can change the reading. Do not measure in a thin layer, in a small cup, or by holding the thermometer in your hand. If the thermometer was stored in a hot truck or a cold box, let it equilibrate with the concrete.

Traps and rule of thumb

A common trap is reading too soon: a thermometer may appear stable after 30 seconds but still be drifting. Another trap is measuring the container wall instead of the concrete, or measuring a sample that sat in the sun. Do not use an infrared surface thermometer for acceptance.

Rule of thumb: 3 in. deep, 3 in. immersion, 3 in. from the side, 2 minutes, read in place. Worked example: after 45 seconds the display shows 72°F, but after the full 2 minutes it stabilizes at 76°F. Record 76°F, not 72°F.

Slump of Hydraulic Cement Concrete

Mold and filling

The slump test uses a standard mold 4 in. (100 mm) across the top, 8 in. (200 mm) across the bottom, and 12 in. (300 mm) high, with a base plate. Dampen the mold and plate, place the mold on a level, rigid surface, and fill in three layers, each about one-third of the volume. Rod each layer 25 times with a 5/8 in. (16 mm) rounded rod. Rod the bottom layer through its full depth; for the upper layers, penetrate about 1 in. (25 mm) into the layer below.

Strike-off and removal

Strike off the top with a trowel, clean the base plate, and remove the mold vertically within 5 ± 2 seconds. Measure the slump immediately as the difference between the mold height and the height of the slumped concrete at the center, to the nearest 1/4 in. (5 mm). Complete filling and rodding within 2.5 minutes. If the concrete shears or collapses, the test is not valid; obtain a new sample.

Traps and worked example

Typical traps are too few strokes, rocking the mold while lifting, lifting at an angle, measuring from the side rather than the center, and testing stale concrete. A very stiff or nonplastic mix may not be suitable for slump.

Rule of thumb: 3 layers, 25 strokes, 5 seconds to lift, 1/4 in. precision. Worked example: mold height is 12 in.; slumped height at the center is 7 3/4 in.; slump = 12 − 7 3/4 = 4 1/4 in.

Density (Unit Weight), Yield, and Gravimetric Air Content

Measurements

Density, unit weight, yield, and gravimetric air content come from one set of measurements. Determine the volume of the measuring bowl by filling it with water and weighing; use that calibrated volume, not a nominal size. Fill the bowl with concrete in layers, consolidate by rodding or vibration as required for the bowl size, strike off, and determine the mass of concrete in the bowl. Density (unit weight) = mass of concrete ÷ volume of bowl.

Calculations

Theoretical density is the total mass of all batch materials divided by their total absolute volume, with no air. Gravimetric air content = [(theoretical density − measured density) ÷ theoretical density] × 100. Yield = total batch mass ÷ measured density. Relative yield = yield ÷ design yield; cement content = cement mass ÷ yield. Keep units consistent, and subtract the empty bowl mass.

Traps and worked example

Traps include using an uncalibrated bowl, guessing the bowl volume, failing to consolidate, and mixing pounds with kilograms. Another trap is reporting air content as a fraction; it is a percentage.

Worked example: bowl volume = 0.25 ft³; concrete mass = 36.0 lb; density = 36.0 ÷ 0.25 = 144 lb/ft³. Theoretical density = 150 lb/ft³. Air = (150 − 144) ÷ 150 × 100 = 4.0%. For a 1,800 lb batch, yield = 1,800 ÷ 144 = 12.5 ft³.

Air Content by the Pressure Method

Pressure meter procedure

The pressure method measures air by compressing the concrete in a sealed bowl and reading the gauge. Fill the bowl in three layers, rod each layer 25 times, tap the sides, strike off, and clean the flange. Clamp the lid, close the valves, and pump to the specified pressure. Tap the gauge gently while pumping and again before reading, then read the air content. The meter must be calibrated and in good condition, with clean seals.

Aggregate correction

The aggregate correction factor accounts for air trapped in the aggregate or for the compressibility of the aggregate. It is determined for the aggregate combination and is subtracted from the meter reading. Do not ignore it, and do not use a correction factor from a different aggregate source. The pressure method is not suitable for highly porous or lightweight aggregates that compress or absorb air.

Traps and worked example

Common traps are a leaking lid, concrete on the flange, not tapping the gauge, and reading before pressure stabilizes. Another trap is using the pressure meter as if it needed no correction.

Rule of thumb: seal clean, tap twice, read once, subtract the correction. Worked example: the gauge reads 6.5%; the aggregate correction factor is 0.8%; air content = 6.5 − 0.8 = 5.7%.

Air Content by the Volumetric Method

Volumetric procedure

The volumetric method measures air by displacing it with water and alcohol in a calibrated meter. Fill the meter with concrete in layers, consolidate each layer, and strike off. Add water and isopropyl alcohol, then roll and invert the meter so the alcohol breaks the air bubbles and the air escapes. Continue until the water level in the graduated neck becomes stable, and read the air content at the bottom of the meniscus. The method gives a direct volume reading and requires no aggregate correction factor.

When to use it

The volumetric method is useful for concrete made with lightweight or porous aggregates, where the pressure method may be unreliable. It is also useful as a field check. The meter must be clean, calibrated, and used with the correct amount of alcohol. The concrete must be representative and must not have lost water before testing.

Traps and worked example

Traps include too little alcohol, insufficient rolling and inverting, reading the top of the meniscus, and failing to tap the meter to release bubbles. Another trap is using a dirty or leaking meter.

Rule of thumb: roll, invert, tap, and wait for a stable level. Worked example: after rolling, the water level rests at the 5.0% mark; the air content is 5.0%. If the level continues to rise, keep rolling; do not read until it is stable.

Making and Curing Concrete Test Specimens in the Field

Molds and filling

Field specimens must represent the concrete and be made promptly. Use clean, properly sized molds: 6 by 12 in. (150 by 300 mm) or 4 by 8 in. (100 by 200 mm). For 6 by 12 in. cylinders, fill in three layers and rod each layer 25 times; for 4 by 8 in. cylinders, fill in two layers and rod each layer 25 times. Use a rounded rod, tap the outside of the mold after each layer to close voids, and strike off the top.

Curing and handling

Initial curing must protect specimens from moisture loss and keep them at 60 to 80°F (16 to 27°C). Remove molds after about 24 hours, then cure in moist conditions at 73.4 ± 3.5°F (23 ± 2°C) for standard curing. Mark specimens for identification, keep them moist, and transport them without shock or freezing. Field-cured specimens are cured at the job site, not in the moist room.

Traps and worked example

Traps include using three layers for a 4 by 8 in. cylinder, too few rod strokes, letting the top dry, and storing cylinders in a hot truck. Another trap is confusing field curing with standard curing.

Rule of thumb: 6 by 12 in. = three layers; 4 by 8 in. = two layers; 25 strokes in every layer. Worked example: a 6 by 12 in. cylinder has a volume of about 0.196 ft³, so three cylinders need about 0.59 ft³ of concrete.

Capping and Compressive Strength Testing of Cylindrical Specimens

Capping

Capped ends must be flat, perpendicular, and parallel so the load is applied uniformly. Use sulfur mortar or another approved capping material, and follow its curing requirements. Keep the cap thin; a thick cap can crush or flow and change the result. The capped end should not depart from perpendicularity by more than about 0.5 degrees. Use a flat capping plate and check the cap with a straightedge.

Compression testing

Measure the cylinder diameter and calculate the cross-sectional area. Center the specimen in the testing machine and apply load at 35 ± 7 psi/s (0.25 ± 0.05 MPa/s) for standard cylinders. Compressive strength = maximum load ÷ cross-sectional area. Report the average of the required specimens and note any unusual fracture pattern.

Traps and worked example

Traps include a cap that is too thick, a tilted cap, an eccentric specimen, and loading too fast. Another trap is using the nominal diameter without checking the actual diameter, or testing a damaged or dry specimen.

Rule of thumb: flat, thin, perpendicular cap; slow, steady load. Worked example: a 6 in. diameter cylinder has an area of π × 3² = 28.27 in². If the maximum load is 85,000 lb, strength = 85,000 ÷ 28.27 = 3,007 psi, reported as about 3,010 psi.

ACI Field Testing I cheat sheet

Quick reference

Sampling Freshly Mixed Concrete

  • ASTM C172 governs sampling; the sample must represent the entire batch and be taken from the middle portion of the discharge, not the first or last material.

  • Use a clean, dampened receptacle; never sample from concrete contaminated by soil, set concrete, or excessive wash water.

  • Collect enough concrete to complete all required field tests and cast specimens; a common minimum is about 1 ft³ (28 L).

  • For a composite sample, combine increments from several portions of the batch and remix before testing; do not test a grab sample as if it were representative.

  • Begin temperature, slump, and air tests promptly after sampling; protect the concrete from sun, wind, and evaporation before testing.

  • Remix each test portion with a shovel before placing it in the test apparatus, but do not add water to make the sample easier to handle.

  • Record batch or truck identity, location, time, and any deviations; field test results are traceable only if sampling is documented.

  • Do not sample from a stationary pile or from a chute after segregation; obtain concrete while it is flowing and homogeneous.

Quick reference

Temperature of Freshly Mixed Concrete

  • ASTM C1064 covers temperature of freshly mixed concrete; use a calibrated thermometer with sufficient immersion depth.

  • Immerse the sensing portion at least 3 in. (75 mm) into the concrete, avoiding contact with the container, and read after at least 2 min or when stable.

  • Report temperature to the nearest 0.5°C (1°F), and compare it with the project specification limits for placing and curing.

  • Measure temperature on a representative sample immediately after sampling; do not let the sample sit in sun or wind.

  • An infrared thermometer measures surface temperature only and is not an acceptable substitute for ASTM C1064 immersion measurement.

  • For large batches or placements, take readings at multiple representative locations if the specification requires it.

  • Thermometer calibration should be verified against a reference thermometer; a damaged or drifting thermometer invalidates results.

  • Temperature affects setting time, strength gain, and air content; record it even when no limit is specified.

Quick reference

Slump of Hydraulic Cement Concrete

  • ASTM C143 slump mold: 12 in. (300 mm) high, 8 in. (200 mm) bottom diameter, and 4 in. (100 mm) top diameter.

  • Place the mold on a firm, level, nonabsorbent base, moisten the mold, and hold it firmly during filling.

  • Fill in three equal layers; rod each layer 25 times with a 5/8 in. (16 mm) bullet-nosed rod, distributing strokes uniformly.

  • Strike off the top, then remove the mold vertically in 5 ± 2 s without twisting or lateral movement.

  • Measure slump immediately as the vertical difference between the original top of the mold and the displaced center of the concrete.

  • Report slump to the nearest 1/4 in. (5 mm); if the concrete shears or collapses, record that condition because the value may not represent true slump.

  • Complete the slump test within 2.5 min after sampling; do not retest a sample that has been standing.

  • Slump is not a measure of workability for all mixtures; very dry or very wet concrete may require a different consistency test.

Quick reference

Density (Unit Weight), Yield, and Air Content (Gravimetric) of Concrete

  • ASTM C138 determines density, yield, and gravimetric air content using a calibrated measure of known volume.

  • Density (unit weight) = mass of concrete in the measure ÷ volume of the measure; report in lb/ft³ or kg/m³.

  • Yield = total mass of the batch ÷ measured unit weight; relative yield = actual yield ÷ design volume.

  • Gravimetric air content = 100 × (1 − measured unit weight ÷ theoretical air-free unit weight).

  • Consolidate the concrete in the measure according to slump: rodding for normal concrete or vibration for low-slump concrete, following C138.

  • Strike off the surface, clean the measure, and determine mass to the required precision; the measure volume must be calibrated.

  • For yield calculations, use the actual total mass of all materials batched, including water and admixtures.

  • Gravimetric air content is less direct than pressure or volumetric methods and depends on an accurate theoretical unit weight.

Quick reference

Air Content of Freshly Mixed Concrete by the Pressure Method

  • ASTM C231 pressure method uses Boyle's law: pressurized air compresses the air voids and the gauge indicates air content.

  • Select a meter and calibration range appropriate for the expected air content and aggregate size.

  • Fill and consolidate the measure per C231, strike off, clean the flange, and clamp the lid to prevent leakage.

  • Apply the specified pressure, tap the meter to stabilize the reading, and read the gauge at the required pressure.

  • Air content = gauge reading − aggregate correction factor; determine the correction factor for the aggregate combination by calibration.

  • The pressure method is not suitable for highly porous or lightweight aggregates without a verified correction.

  • Check the meter for leakage and proper water level; a leaking or dirty meter produces false low or high readings.

  • Record the gauge pressure, reading, correction factor, and final air content.

Quick reference

Air Content of Freshly Mixed Concrete by the Volumetric Method

  • ASTM C173 volumetric method measures air by removing it from a known concrete volume and reading the water-level drop.

  • Fill the measuring bowl, add water, and seal the meter; invert and roll the meter to displace air from the concrete.

  • Repeat agitation and settling until the air volume reading stabilizes; trapped air must be fully released.

  • Read air content directly from the graduated neck, usually to the nearest 0.1%.

  • The volumetric method is useful for concrete made with dense aggregate and for field checks where pressure equipment is unavailable.

  • Do not use the volumetric method for concrete that is too stiff to agitate or for aggregate that releases gas.

  • Keep the meter clean and check the seal; leakage or residual air causes inaccurate readings.

  • Record the final reading and any aggregate correction required by the procedure.

Quick reference

Making and Curing Concrete Test Specimens in the Field

  • ASTM C31 covers making and curing field specimens; use molds and rodding equipment that meet the standard.

  • Cylinder size: 6 x 12 in. (150 x 300 mm) for nominal maximum aggregate up to 2 in.; 4 x 8 in. (100 x 200 mm) for smaller aggregate as permitted.

  • For 6 x 12 in. cylinders, fill in three layers and rod each layer 25 times; for 4 x 8 in. cylinders, use two layers and 25 strokes per layer.

  • Tap the outside of the mold 10 to 15 times after each layer to release entrapped air, then strike off the top.

  • Initial cure specimens at 60 to 80°F (16 to 27°C) and protect from moisture loss for 24 ± 8 h before demolding.

  • After demolding, cure specimens at 73.5 ± 3.5°F (23 ± 2°C) in limewater or a moist room until the test age.

  • Mark specimens clearly and transport them only after they are strong enough; protect them from vibration, freezing, and drying.

  • Do not use specimens with honeycombing, voids, or damaged ends for acceptance strength testing.

Quick reference

Capping and Compressive Strength Testing of Cylindrical Specimens

  • ASTM C617 covers capping cylindrical specimens; caps must be perpendicular to the cylinder axis and provide a smooth, flat bearing surface.

  • Sulfur mortar or cement paste caps should be thin and sound; excessive thickness or voids can reduce measured strength.

  • ASTM C39 compression test: measure specimen dimensions, center it in the testing machine, and apply load without shock.

  • Compressive strength = maximum load ÷ cross-sectional area; report to the required precision.

  • Use the specified loading rate for the cylinder size; do not adjust the rate to chase an expected result.

  • Reject or qualify specimens with damaged ends, improper caps, or visible defects before testing.

  • Record fracture pattern, age, dimensions, maximum load, and calculated strength.

  • Testing machine calibration and proper bearing block alignment are essential for valid strength results.

ACI Field Testing I key terms

composite sample

A test sample created by combining two or more portions of concrete taken at different times or locations during discharge of the same batch, so the result represents the whole batch rather than one spot.

Related: sample reduction, elapsed time limits
sample size

The minimum quantity of fresh concrete collected for testing. For strength specimens and most field tests, standards require at least 1 cubic foot (about 28 liters) so enough material exists for every required test.

Related: composite sample, standard cylinder
sampling from stationary mixer

Collecting concrete from a stationary mixer by discharging the middle portion of the batch into a clean container, setting aside the very first and very last material that may be unrepresentative.

Related: composite sample, remixing the sample
sample reduction

Reducing a large sample to a smaller one without changing its proportions, typically by remixing it on a clean, flat, nonabsorbent surface and quartering or splitting so each portion stays representative.

Related: composite sample, remixing the sample
elapsed time limits

Rules governing how long sampling and testing may take: the composite sample is gathered over no more than 15 minutes, and testing begins within 5 minutes after the sample is obtained.

Related: composite sample, temperature reading
remixing the sample

Thoroughly mixing a sample with a shovel or scoop before each test portion is taken, so aggregate and paste stay evenly distributed after transport and the sample does not segregate.

Related: sample reduction, composite sample
thermometer verification

Checking a field thermometer against a reference device or known temperatures at regular intervals to confirm its readings are within 1 degree F, since unverified readings make temperature records unreliable.

Related: temperature reading, immersion depth
immersion depth

The distance the thermometer is pushed below the concrete surface, at least 3 inches (75 mm), ensuring the sensing element is surrounded by fresh concrete rather than air or surface material.

Related: temperature reading, thermometer verification
temperature reading

The measurement of freshly mixed concrete temperature, taken after the thermometer sits in place at least 2 but no more than 5 minutes and read to the nearest 1 degree F.

Related: immersion depth, thermometer verification
slump

A measure of the consistency or workability of fresh concrete, expressed as the vertical distance the freshly molded sample settles after the cone is lifted away.

Related: slump cone, slump measurement
slump cone

The metal mold used to form the slump specimen, 12 inches tall with an 8-inch bottom and 4-inch top diameter, fitted with a base plate and foot pieces.

Related: tamping rod, slump
tamping rod

A round, smooth steel rod 5/8 inch in diameter and about 24 inches long with a rounded tip, used to consolidate concrete in the slump cone, unit weight measure, and cylinder molds.

Related: slump cone, rodding layers
slump measurement

The drop from the top of the cone to the displaced original center of the slumped specimen, measured to the nearest 1/4 inch (5 mm) after the concrete comes to rest.

Related: slump, shear slump
shear slump

A slump result where one side of the specimen slides down more than the other, indicating the concrete is not uniform; the test may need to be repeated on a new sample.

Related: slump measurement, slump
unit weight

The mass of fresh concrete per unit of volume, determined by filling a calibrated measure, consolidating it, striking off the top, and dividing the mass of concrete by the measure's volume.

Related: measure calibration, yield
yield

The actual volume of concrete produced by a batch, calculated as the total mass of all materials batched divided by the measured unit weight of the fresh concrete.

Related: unit weight, relative yield
gravimetric air content

Air content computed by comparing the measured density of fresh concrete with its theoretical air-free density; the difference divided by the theoretical density, times 100, gives percent air.

Related: theoretical density, unit weight
measure calibration

Determining the exact volume of a container by filling it with water at a known temperature and weighing it, so the volume used in unit weight calculations is accurate.

Related: unit weight, strike-off
theoretical density

The density concrete would have with no air voids, computed from batch proportions by summing the absolute volumes of cement, water, aggregates, and admixtures.

Related: gravimetric air content, unit weight
strike-off

Removing excess concrete above the rim of the measure or mold with a straightedge, using a sawing motion and then a flat finish, so the top surface is level with the rim.

Related: unit weight, measure calibration
relative yield

The ratio of the actual yield of a batch to its designed volume, showing whether the batch produced more or less concrete than planned for the given materials.

Related: yield, unit weight
pressure air meter

A device that measures air content by sealing a concrete sample in a vessel, applying air pressure above the water, and reading the gauge change that corresponds to compressible air in the concrete.

Related: aggregate correction factor, pressure meter calibration
aggregate correction factor

A small percentage subtracted from the meter reading to correct for air trapped in the pores of the aggregate, established beforehand by testing representative aggregate samples with the same meter.

Related: pressure air meter, volumetric air meter
pressure meter calibration

The process of verifying a pressure air meter using known volumes or the manufacturer's procedure, so gauge readings correctly translate pressure change into percent air content.

Related: pressure air meter, aggregate correction factor
volumetric air meter

An apparatus that measures air content by filling a calibrated vessel with concrete and water, adding alcohol, and agitating until the water level shows the volume of air removed from the sample.

Related: isopropyl alcohol, aggregate correction factor
isopropyl alcohol

A liquid added to the volumetric air meter to break surface tension and reduce foaming, so the water level can be read clearly and the air volume measured accurately.

Related: volumetric air meter, rolling and agitating the meter
rolling and agitating the meter

Inverting and rolling the volumetric meter on a flat surface after adding alcohol, repeating the agitation until the water level stops changing and all released air has collected at the top.

Related: volumetric air meter, isopropyl alcohol
standard cylinder

A cylindrical test specimen of concrete, commonly 6 by 12 inches or 4 by 8 inches, cast in a mold, cured under controlled conditions, and later tested in compression.

Related: cylinder mold, rodding layers
rodding layers

Consolidating concrete in a mold by pushing the tamping rod a set number of times per layer, commonly 25 strokes in each of three layers for 6-by-12-inch cylinders.

Related: tamping rod, standard cylinder
cylinder mold

A single-use or reusable cylindrical form made of material that does not absorb water or react with concrete, oiled lightly before filling and sealed so it holds its shape.

Related: standard cylinder, initial curing
initial curing

Storage of freshly cast specimens at 60 to 80 degrees F in a moist environment for the first day, protecting them from freezing, drying, and vibration until the molds are removed.

Related: standard curing, cylinder mold
standard curing

Moist curing of hardened specimens in limewater or a moist room at about 73 degrees F until the age of test, so strength results are comparable to reference laboratory conditions.

Related: initial curing, compressive strength
capping compound

A stiff material such as sulfur mortar or gypsum paste applied to a cylinder end to create a flat, smooth bearing surface; it must reach adequate strength before the specimen is tested.

Related: cap planeness, compressive strength
cap planeness

The flatness of a capped cylinder end, required to be within about 0.002 inch across the cap so the load is applied uniformly and the specimen is not loaded eccentrically.

Related: capping compound, fracture pattern
compressive strength

The maximum compressive load a concrete specimen carries per unit of cross-sectional area before failure, usually reported in psi or MPa at a specified age.

Related: loading rate, test cylinder area
loading rate

The speed at which the testing machine applies load, held within a specified range such as 35 psi per second, because faster or slower loading changes the measured strength.

Related: compressive strength, spherical seat
fracture pattern

The shape of a cylinder's break after compression testing, such as cone, cone and shear, or columnar, recorded because unusual patterns may point to capping or machine problems.

Related: cap planeness, compressive strength
spherical seat

The machine component that aligns with the top of the specimen so load is applied evenly, seated properly and kept clean to avoid eccentric loading during the test.

Related: loading rate, compressive strength
test cylinder area

The cross-sectional area of a cylinder, computed from a diameter measured near mid-height rather than the nominal size, used to convert failure load into compressive stress.

Related: compressive strength, loading rate

ACI Field Testing I study plan

8 weeks · About 6 hours per week

Week 1

Sampling Freshly Mixed Concrete & Temperature of Freshly Mixed Concrete

  • Execute the full sampling sequence - obtain, remix, and reduce - on a practice batch and verbalize the reason for each action as you take it

  • Determine the minimum sample volume required for slump, air content, density, and strength specimens, and state the consequence of undersizing each one

  • Measure the temperature of freshly mixed concrete with a calibrated thermometer using the correct immersion depth, minimum immersion time, and reading interval

  • Identify the field conditions that invalidate a temperature reading and describe the corrective action for each

Your checkpoint

A one-page sampling and temperature checklist written from memory, then scored against the written procedure with zero critical omissions.

Week 2

Slump of Hydraulic Cement Concrete & Density (Unit Weight), Yield, and Air Content (Gravimetric) of Concrete

  • Perform a slump test start to finish with correct mold filling, rodding pattern, lift timing, and measurement to the nearest 5 mm (1/4 in.)

  • Distinguish a true slump from a shear slump and a collapse, and state when the result must be discarded and the test repeated

  • Calculate density, yield, cement content, and gravimetric air content from a given set of field masses and mold volumes

  • Compare the computed yield against the design yield and decide whether the batch falls within the acceptance tolerance

  • Record all slump, density, and yield values on a field data sheet with correct units and significant figures

Your checkpoint

A worked calculation sheet containing two complete density/yield/air problems solved to within 1% of the reference answer, plus one fully documented slump record.

Week 3

Making and Curing Concrete Test Specimens in the Field

  • Collect and remix a representative sample, then mold standard cylinders using the correct number of layers, rod strokes, and strike-off technique

  • Apply the proper consolidation method for the measured slump and identify when vibration replaces rodding

  • Label, protect, and transport specimens so that initial curing temperature and moisture requirements are met

  • Complete a curing log that tracks specimen identity, initial and final curing conditions, and test date

Your checkpoint

A complete specimen log for six molded practice cylinders with every field filled in and no missing traceability data.

Week 4

Capping and Compressive Strength Testing of Cylindrical Specimens

  • Prepare cylinder ends by capping so that the cap is perpendicular to the axis and within the allowed thickness and planeness limits

  • Select the appropriate capping material or pad for a given strength range and justify the choice

  • Compute compressive stress from the recorded peak load and measured diameter, and apply the correct unit conversion

  • Classify the mode of fracture for a tested cylinder and state whether the result is acceptable

  • List the machine verification checks that must be confirmed before a test result is considered valid

Your checkpoint

Two fully worked strength calculations with fracture-pattern classification, plus a cap-acceptance checklist applied to four practice specimens.

Week 5

Air Content of Freshly Mixed Concrete by the Pressure Method

  • Zero and calibrate a pressure-type air meter and confirm that the gauge holds pressure without decay

  • Determine the aggregate correction factor for a given aggregate combination and apply it correctly to the meter reading

  • Perform the complete pressure-method test on a prepared sample, recording initial and final pressure readings

  • Troubleshoot at least five common causes of erratic or inconsistent pressure-meter results and describe the fix for each

Your checkpoint

An aggregate correction factor worksheet for two aggregate combinations plus a completed pressure-meter field data sheet with the corrected air content shown.

Week 6

Air Content of Freshly Mixed Concrete by the Volumetric Method

  • Perform the volumetric air-content test with correct reagent addition, pressure vessel agitation, and reading technique

  • Convert the volumetric reading into an air content value and determine whether it meets the specified tolerance

  • Compare pressure-method and volumetric results on the same sample and explain any discrepancy larger than the permitted difference

  • State the restrictions that make the volumetric method unsuitable for certain concretes, such as those with lightweight or highly porous aggregate

Your checkpoint

A side-by-side comparison table of pressure and volumetric air results on the same simulated mixture, with every difference greater than 0.5% explained in writing.

Week 7

Slump of Hydraulic Cement Concrete & Air Content of Freshly Mixed Concrete by the Pressure Method & Air Content of Freshly Mixed Concrete by the Volumetric Method

  • Trace how sample handling and remixing affect measured slump and air content, predicting the direction of bias for each error

  • Build a retest plan for a scenario in which air content is within specification but early strength is low

  • Reproduce from memory the air content acceptance limits for each exposure class and the tolerances that apply to slump

  • Explain how aggregate correction factor errors propagate into the reported air content and how to detect them

Your checkpoint

A troubleshooting decision tree covering eight field error scenarios, each with a detection step, a correction, and the record that must be kept.

Week 8

Sampling Freshly Mixed Concrete & Temperature of Freshly Mixed Concrete & Slump of Hydraulic Cement Concrete & Density (Unit Weight), Yield, and Air Content (Gravimetric) of Concrete & Air Content of Freshly Mixed Concrete by the Pressure Method & Air Content of Freshly Mixed Concrete by the Volumetric Method & Making and Curing Concrete Test Specimens in the Field & Capping and Compressive Strength Testing of Cylindrical Specimens

  • Complete two full-length timed practice exams under exam-day conditions

  • Review every missed item and write the underlying rule or calculation that caused the error

  • Recompute the numerical items from domains 4, 5, and 8 without reference material until each is correct twice in a row

  • Recite the field procedures for all eight domains in sequence from memory as a final retention check

Your checkpoint

A written error log for every missed question across both practice exams, with each error traced to a specific rule and re-tested.

Milestones

Week 2: Score at least 80% on a 15-question closed-note quiz on sampling, temperature, and slump, and complete a slump test with no procedural errors observed.

Week 4: Score at least 80% on a 25-question cumulative quiz covering domains 1, 2, 3, 4, 7, and 8, and solve both density/yield and compressive-strength problems correctly without notes.

Week 6: Score at least 85% on a 20-question quiz covering all three air-content methods and compute a corrected aggregate air content in under 10 minutes.

Week 8: Score at least 85% on two full-length timed practice exams, including one closed-note attempt, with a completed error log for every missed item.

ACI Field Testing I exam day

Your checklist

Government-issued photo ID

Bring an unexpired photo ID. Acceptable forms and name-matching requirements vary by provider, so confirm with the provider in advance.

Registration or admission confirmation

Bring the confirmation email, admission letter, or registration number the provider issued. Save a digital copy as backup.

Non-programmable calculator

Bring a basic calculator for written-exam calculations. Confirm with the provider whether calculators are permitted and what types are allowed.

No. 2 pencils, eraser, and pen

Pack several sharpened pencils and a good eraser for the written exam, plus a pen for any sign-in forms.

Personal protective equipment

Bring a hard hat, safety glasses, work gloves, and safety-toe boots. Check the provider’s PPE requirements because site rules may add items.

Work clothes suitable for concrete field testing

Wear clothes that can get wet, dusty, or stained. Avoid loose sleeves or jewelry that could catch on equipment.

Watch or timer

A wristwatch or standalone timer is useful for timed steps. Confirm with the provider whether phone timers are allowed in the testing area.

Directions, parking, and arrival information

Confirm the exact testing location, parking options, and reporting time with the provider. Plan a backup route.

Water and a light snack

Bring water and a snack for breaks. Confirm with the provider whether food and drink are allowed in the waiting area.

Review plan for ASTM procedures and calculations

Do a final review of sampling, slump, air content, unit weight, temperature, and cylinder fabrication steps. Do not bring unauthorized notes into the exam room.

Plan the day

Final 72 hours

Confirm your registration status, exam location, reporting time, and required PPE with the provider. Resolve any discrepancy immediately.

Final 72 hours

Review the ASTM test methods and your ACI workbook. Practice the sequence for slump, air content, unit weight, temperature, and cylinder making, including required timing and acceptance criteria.

Final 72 hours

Inspect your PPE and work clothes. Replace damaged safety glasses, worn gloves, or boots that do not meet the provider’s requirements.

Final 72 hours

Plan travel, parking, and a backup route. Confirm whether you need cash or a card for parking.

24 hours before

Pack your bag: ID, registration confirmation, pencils, eraser, pen, calculator, PPE, work clothes, watch, water, and snack.

24 hours before

Re-read key calculation steps and acceptance criteria. Avoid cramming new material; focus on procedures you already know.

24 hours before

Set two alarms, check the weather, and confirm your departure time. Aim to arrive early rather than on time.

24 hours before

Get a full night’s sleep and avoid alcohol. Fatigue hurts both written-exam focus and hands-on performance.

Morning of the exam

Eat breakfast and hydrate. Bring water for breaks if permitted.

Morning of the exam

Arrive at the site early, allowing time for check-in, ID verification, and storing personal belongings as directed.

Morning of the exam

Present your ID and confirmation, listen to the examiner’s instructions, and ask where to wait and what to do if you need a restroom break.

During the test

For the written exam, answer the questions you know first, mark uncertain items, and return to them if time allows. Keep track of time.

During the test

For the performance exam, follow the examiner’s directions, use the required PPE, and perform each step in the correct order. If a procedural instruction is unclear, ask the examiner whether clarification is allowed before proceeding.

During the test

Record and report results as required, clean equipment between tests if directed, and do not discuss exam content with other candidates during breaks.

Rules to check

  • Bring a government-issued photo ID. Confirm with the provider which ID forms are acceptable and whether the name must match your registration exactly.

  • Do not communicate with other candidates during the written or performance exam. Follow the examiner’s instructions about where to stand, what to touch, and when to speak.

  • Electronic devices: confirm the provider’s policy before exam day. Unless told otherwise, silence and store phones and smartwatches out of reach during testing.

  • Breaks: confirm the break policy with the provider. Do not leave the testing area during a timed section without the examiner’s permission.

  • Scoring: written and performance portions may both require a passing result. Confirm the passing score, retest policy, and score-report timing with the provider.

  • Reference materials: confirm what, if anything, may be brought into the exam. Do not rely on notes, handwritten charts, or phone references unless the provider explicitly permits them.

  • Safety and conduct: wear the required PPE, use equipment as directed, report hazards immediately, and stop work if the examiner calls a halt.

  • Integrity: no cheating, no sharing answers, and no photographing exam materials. Follow all provider rules; unclear situations should be resolved by asking the examiner before acting.

ACI Field Testing I FAQ

How many ACI Field Testing I practice questions are available?

The practice set has 200 ACI Field Testing I questions. Each one includes the choices, the correct answer, and an explanation, and the set is free to read with no signup.

How many ACI Field Testing I flashcards are available?

The flashcard set has 32 ACI Field Testing I cards. Each card shows the term and its definition.

Which topics does the ACI Field Testing I study material cover?

The ACI Field Testing I study material has 8 sections, including Sampling Freshly Mixed Concrete, Temperature of Freshly Mixed Concrete, and Slump of Hydraulic Cement Concrete.

What format facts does the catalog list for the ACI Field Testing I exam?

The catalog lists these item types: multiple choice and performance (hands-on) test for the ACI Field Testing I exam.